A collector for fine-grained molybdenite, its preparation method and application
By compounding hydrocarbon oil collectors and optimizing the flotation process, the problem of difficult flotation of fine-grained molybdenite was solved, achieving efficient recovery and cost reduction, and improving the grade and recovery rate of molybdenum ore.
Patent Information
- Application Number
- CN202410770074.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-14
AI Technical Summary
Traditional non-polar hydrocarbon oil collectors are ineffective in improving the floatability of fine molybdenite particles, leading to difficulties in molybdenum ore flotation, especially in high-muddy, low-grade fine-grained molybdenite ore with low recovery efficiency.
A compound hydrocarbon oil collector, including pyrolysis oil, 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2], and kerosene, is used in the flotation process of fine-grained molybdenite after ultrasonic extraction and constant-temperature water bath treatment. The flotation process is optimized by combining it with modifiers such as water glass and calcium oxide to improve the recovery rate.
It has achieved efficient flotation for recovering high-muddy, low-grade, fine-grained molybdenite, improving molybdenum ore grade and recovery rate, reducing reagent usage and beneficiation costs, increasing molybdenum grade by 0.5–0.62 percentage points, and recovery rate by 10–12 percentage points.
Smart Images

Figure CN118594776B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a collector for fine-grained molybdenite, its preparation method, and its application, belonging to the field of flotation reagent technology in mineral processing. Background Technology
[0002] Molybdenum, as a rare metal, is playing an increasingly important role in the national economy due to its excellent performance. Therefore, the rational development and utilization of molybdenite resources is particularly important. Molybdenite is the most widely distributed molybdenum mineral and also the most crucial molybdenum resource. However, with continuous industrial development, the demand for molybdenum has gradually increased, leading to the large-scale mining of molybdenum resources. This has resulted in a gradual decrease in molybdenum ore, especially high-grade molybdenum ore, and the ore now exhibits characteristics of being low-grade, fine-grained, and impure. To meet industrial needs, the recovery and utilization of low-grade, fine-grained molybdenum ore is receiving widespread attention.
[0003] Hydrocarbon oil collectors, such as kerosene, diesel oil, and transformer oil, are commonly used in the flotation of molybdenite. However, traditional non-polar hydrocarbon oil collectors are ineffective in improving the floatability of fine-grained molybdenite particles, leading to difficulties in molybdenum flotation. It is well known that the surface of molybdenite is non-polar and hydrophobic, while its edges are polar and hydrophilic. As the particle size of molybdenite decreases, the face-to-edge ratio decreases, resulting in a decline in molybdenite flotation performance. To address the problem of ineffective recovery of fine-grained molybdenite, composite collectors have become an effective method for improving molybdenum flotation recovery in recent years. The combination of polycyclic aromatic hydrocarbons (PAHs) and kerosene can improve the flotation recovery rate of molybdenite of different particle sizes. Therefore, determining a reasonable reagent system and process flow is crucial for the development and utilization of molybdenite resources. Summary of the Invention
[0004] To address the problems existing in the prior art, this invention provides a compound hydrocarbon oil collector for fine-grained molybdenite, its preparation method, and its flotation application on high-muddy, low-grade fine-grained molybdenite. This compound hydrocarbon oil collector exhibits excellent selectivity and flotation recovery effect on high-muddy, low-grade fine-grained molybdenite; moreover, the preparation method of this reagent is simple and feasible; the flotation method is convenient, and under suitable flotation reagent regime and flotation process conditions, it achieves good flotation recovery effect on high-muddy, low-grade fine-grained molybdenite.
[0005] This invention is achieved through the following technical solution:
[0006] The collector of the present invention is a compound hydrocarbon oil collector, the components of which include pyrolysis oil, 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2] and kerosene. The compound hydrocarbon oil collector is used to collect fine-grained molybdenite with high mud content and low grade.
[0007] The preparation method of the compound hydrocarbon oil collector of the present invention is as follows:
[0008] Pyrolysis oil and 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2] were mixed in a mass ratio of 7:20 to 9:20 and then extracted with ultrasound for 1 hour. The mixture was then placed in a constant temperature water bath and allowed to stand for 2 hours. The extract was then collected and combined with kerosene in a 1:3 ratio to form the compound hydrocarbon oil collector.
[0009] The application of collectors for fine-grained molybdenite in the collection of high-muddy, low-grade fine-grained molybdenite employs a flotation process of one rougher, two cleaners, and three scavengers, as detailed below:
[0010] (1) Grind the raw ore to a particle size of less than 0.074 mm by mass, accounting for 60-65%, adjust the slurry concentration to 30-45%, and then add the modifier, the compound hydrocarbon oil collector and the frother to the slurry for a roughing operation to obtain molybdenite roughing concentrate and molybdenite roughing tailings.
[0011] (2) After regrinding the molybdenite concentrate from step (2) to 90% of the content of -0.038mm, it is put into flotation. Add modifier and frother to carry out two cleaning operations. The cleaning operation I yields the cleaning I concentrate and the cleaning I middlings. Add modifier and frother to the cleaning I concentrate to carry out the cleaning II operation to obtain the molybdenite concentrate and the cleaning II middlings. The cleaning I middlings are returned to the roughing operation, and the cleaning II middlings are returned to the cleaning I operation to form a closed loop.
[0012] (3) Add the modifier, the compound hydrocarbon oil collector and the frother to the molybdenite roughing tailings from step (1), and perform three scavenging operations. The middlings from the three scavenging operations are mixed and returned to the roughing operation to form a closed loop to obtain tailings.
[0013] The application of collectors for fine-grained molybdenite in the collection of fine-grained molybdenite with high mud content and low grade, wherein the modifiers in steps (1) to (3) are calcium oxide and water glass, and the foaming agent is MIBC.
[0014] The application of collectors for fine-grained molybdenite in the collection of high-mud-content, low-grade fine-grained molybdenite is as follows:
[0015] The dosages of the reagents in step (1) are as follows: 400-1000 g / t of calcium oxide as modifier, 150-450 g / t of water glass, 60-80 g / t of compound hydrocarbon oil collector, and 48-60 g / t of MIBC foaming agent; the dosages of the reagents in step (2) are as follows: 100-200 g / t of calcium oxide as modifier for Selective I, 15-80 g / t of water glass, and 0-10 g / t of MIBC foaming agent; 0-100 g / t of calcium oxide as modifier for Selective II, 20-40 g / t of water glass, and 0-6 g / t of MIBC foaming agent; the dosages of the reagents in step (3) are as follows: 75-120 g / t of water glass for Scavenging I, 20-40 g / t of compound collector, and MIBC foaming agent. The pyrolysis oil is produced by high-temperature cracking of carbonaceous organic matter. Its main components are a large amount of aliphatic hydrocarbons, aromatics, and cycloalkanes. It has high collecting and selectivity, and its foaming properties can reduce the amount of foaming agent required to some extent. The additives for scavenging II include calcium oxide (100-200g / t), water glass (15-80g / t), compound collector (10-25g / t), and frother MIBC (10-20g / t).
[0016] [AMIM][NTF2] is an ionic liquid composed of 1-allyl-3-methylimidazolium cation and bis(trifluoromethanesulfonyl)imide anion. It has high stability, non-toxicity, good solubility and tunable structural properties. Its unique molecular structure gives it high surface activity in aqueous solution, making it a new type of green media material. Due to the special structure of the benzene ring in aromatic hydrocarbons, it reacts readily with ionic liquids, promoting the separation of aromatic hydrocarbons.
[0017] The pyrolysis oil was extracted with [AMIM][NTF2] at a mass ratio of 2:5 to extract the effective components such as phenanthrene and naphthalene containing benzene rings, forming a [AMIM][NTF2] solution containing a large number of compounds with benzene rings. These effective components are beneficial to the adsorption of fine molybdenite particles, increase the adsorption energy of the hydrophilic surface at the edge of molybdenite, reduce the surface electronegativity of molybdenite, improve the hydrophobicity of the molybdenite surface, and improve the flotation of fine molybdenite particles.
[0018] Kerosene, as a common non-polar hydrocarbon oil collector for molybdenite, can be adsorbed onto the surface of fine-grained molybdenite through van der Waals forces during the collection process, thereby increasing the hydrophobicity of molybdenite.
[0019] A solution containing polycyclic aromatic hydrocarbons (PAHs) [AMIM][NTF2] is compounded with kerosene. Under the combination of PAHs and kerosene, PAHs are adsorbed on the hydrophilic surface of molybdenite edge, while kerosene is adsorbed on the surface of molybdenite. This is beneficial to improving the separation efficiency of fine-grained molybdenite, improving the flotation of fine-grained molybdenite, and increasing the flotation efficiency of fine-grained molybdenite.
[0020] By adding water glass, the muddy material in the slurry is dispersed, reducing its encapsulation of the target mineral and minimizing its impact on flotation. Furthermore, by adding the compound collectors pyrolysis oil-[AMIM][NTF2] and kerosene, the target mineral in low-grade molybdenite is efficiently enriched, thereby improving the grade and recovery rate of molybdenite flotation.
[0021] In step (1), the content of quartz, a mineral in molybdenite vein, is between 40% and 65%.
[0022] The beneficial effects of this invention are:
[0023] (1) The compound collector used in this invention achieves efficient flotation recovery of the target mineral, high mud content, low grade, fine-grained molybdenite, effectively improving the grade and recovery rate of molybdenite and reducing the loss of molybdenum resources.
[0024] (2) The compound collector used in this invention achieves efficient flotation recovery of molybdenite, reduces reagent usage, and lowers separation costs. Under the same conditions, compared with the use of a single collector, the molybdenum grade is increased by 0.5 to 0.62 percentage points and the molybdenum recovery rate is increased by 10 to 12 percentage points. Attached Figure Description
[0025] Figure 1 This is a simplified flotation process diagram of the present invention. Detailed Implementation
[0026] To make the objectives, technical solutions, and beneficial effects of this invention clearer, the technical solutions of this invention will be described in detail below. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are all within the scope of protection of this invention.
[0027] Example 1: The collector in this example is a compound hydrocarbon oil collector, whose components include pyrolysis oil, 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2], and kerosene. This compound hydrocarbon oil collector is used to collect fine-grained molybdenite with high clay content and low grade. The preparation method of the compound hydrocarbon oil collector is as follows:
[0028] The pyrolysis oil and 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2] were mixed at a mass ratio of 7:20 and extracted with ultrasound for 1 hour. The mixture was then placed in a constant temperature water bath and allowed to stand for 2 hours. The extract was then collected and combined with kerosene at a ratio of 1:3 to form the compound hydrocarbon oil collector.
[0029] The collector for this fine-grained molybdenite was applied to the collection of high-muddy, low-grade fine-grained molybdenite using a flotation process of one rougher, two cleaners, and three scavengers, such as... Figure 1 As shown, the details are as follows:
[0030] (1) Grind high-mud-content, low-grade fine-grained molybdenite to a particle size of less than 0.074 mm by mass, accounting for 60%, and adjust the pulp concentration to 35%; wherein, the Mo grade is 0.015% and the quartz content is 62.66%; then add 400 g / t of calcium oxide, 150 g / t of water glass, 80 g / t of compound hydrocarbon oil collector, and 60 g / t of frother MIBC to the pulp in sequence, and carry out one roughing operation to obtain molybdenite roughing concentrate and molybdenite roughing tailings;
[0031] (2) After regrinding the molybdenite concentrate from step (1) to 90% of the sample size (-0.038 mm), the sample is fed into flotation. 200 g / t of calcium oxide, 80 g / t of water glass, and 10 g / t of MIBC are added as modifiers. The sample is then subjected to cleaning operation I to obtain cleaning concentrate I and cleaning middlings I. The cleaning middlings I are returned to the pulp conditioning process and fed into the roughing process. The cleaning concentrate I is then subjected to cleaning operation II. 100 g / t of calcium oxide, 40 g / t of water glass, and 6 g / t of MIBC are added as modifiers. The cleaning operation II yields cleaning concentrate II and cleaning middlings II. The cleaning middlings II are returned to the pulp conditioning process and fed into cleaning operation I. After one roughing, two cleaning, and three scavenging processes, the molybdenite concentrate is obtained.
[0032] (3) Add 100g / t of water glass, 40g / t of compound collector, and 40g / t of frother MIBC to the molybdenite tailings from step (1) in sequence, and perform scavenging operation I to obtain scavenging I middlings and scavenging I tailings. The scavenging I middlings are returned to the roughing operation. Add 200g / t of calcium oxide, 80g / t of water glass, 25g / t of compound collector, and 20g / t of frother MIBC to the scavenging I tailings, and perform scavenging operation II to obtain scavenging II middlings and scavenging II tailings. The scavenging II middlings are returned to the roughing operation. Add 40g / t of water glass, 17.5g / t of compound collector, and 20g / t of frother MIBC to the scavenging II tailings, and perform scavenging operation III to obtain scavenging III middlings and scavenging III tailings. The scavenging III middlings are returned to the roughing operation. The scavenging III tailings are the final tailings.
[0033] In this embodiment, the molybdenite concentrate has a molybdenum grade of 1.20% and a molybdenum recovery rate of 74.56%.
[0034] Comparative Example 1: The steps in this example are the same as in Example 1, except that a single collector, kerosene, is used as the collector, and the amount of reagent used is the same as in Example 1. The molybdenite concentrate obtained in this comparative example has a molybdenite grade of 0.58% and a molybdenum recovery rate of 63.35%.
[0035] Example 2: The collector in this example is the same as in Example 1, except that the mass ratio of pyrolysis oil to 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2] is 9:20. This collector for fine-grained molybdenite is applied to collect high-muddy, low-grade fine-grained molybdenite using a flotation process of one rougher, two cleaners, and three scavengers, as detailed below:
[0036] (1) Grind high-mud-content, low-grade fine-grained molybdenite to a particle size of less than 0.074 mm by mass, accounting for 65%, and adjust the pulp concentration to 30%; wherein, the Mo grade is 0.015% and the quartz content is 62.66%; then add 1000 g / t of calcium oxide, 200 g / t of water glass, 60 g / t of compound hydrocarbon oil collector, and 48 g / t of frother MIBC to the pulp in sequence, and carry out one roughing operation to obtain molybdenite roughing concentrate and molybdenite roughing tailings;
[0037] (2) After regrinding the molybdenite concentrate from step (1) to 90% of the sample size (-0.038 mm), the sample is fed into flotation. 100 g / t of calcium oxide, 15 g / t of water glass, and 5 g / t of MIBC are added as modifiers. The sample is then subjected to cleaning operation I to obtain cleaning concentrate I and cleaning middlings I. The cleaning middlings I are returned to the pulp conditioning process and fed into the roughing process. The cleaning concentrate I is then subjected to cleaning operation II. 50 g / t of calcium oxide, 20 g / t of water glass, and 3 g / t of MIBC are added as modifiers. The cleaning operation II yields cleaning concentrate II and cleaning middlings II. The cleaning middlings II are returned to the pulp conditioning process and fed into cleaning operation I. After one roughing, two cleaning, and three scavenging processes, the molybdenite concentrate is obtained.
[0038] (4) Add 120g / t of water glass, 30g / t of compound collector, and 30g / t of frother MIBC to the molybdenite tailings from step (1) in sequence, and perform scavenging operation I to obtain scavenging I middlings and scavenging I tailings. The scavenging I middlings are returned to the roughing operation. Add 150g / t of calcium oxide, 60g / t of water glass, 20g / t of compound collector, and 15g / t of frother MIBC to the scavenging I tailings, and perform scavenging operation II to obtain scavenging II middlings and scavenging II tailings. The scavenging II middlings are returned to the roughing operation. Add 30g / t of water glass, 20g / t of compound collector, and 10g / t of frother MIBC to the scavenging II tailings, and perform scavenging operation III to obtain scavenging III middlings and scavenging III tailings. The scavenging III middlings are returned to the roughing operation. The scavenging III tailings are the final tailings.
[0039] In this embodiment, the molybdenite concentrate has a molybdenum grade of 1.27% and a molybdenum recovery rate of 73.41%.
[0040] Example 3: The collector in this example is the same as in Example 1, except that the mass ratio of pyrolysis oil to 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2] is 8:20. This collector for fine-grained molybdenite is applied to collect high-muddy, low-grade fine-grained molybdenite using a flotation process of one rougher, two cleaners, and three scavengers, as detailed below:
[0041] (1) Grind high-mud-content, low-grade fine-grained molybdenite to a particle size of less than 0.074 mm by mass, accounting for 70%, and adjust the pulp concentration to 45%; wherein, the Mo grade is 0.015% and the quartz content is 62.66%; then add 800 g / t of calcium oxide, 450 g / t of water glass, 70 g / t of compound hydrocarbon oil collector, and 50 g / t of frother MIBC to the pulp in sequence, and carry out one roughing operation to obtain molybdenite roughing concentrate and molybdenite roughing tailings;
[0042] (2) After regrinding the molybdenite concentrate from step (1) to 90% of the sample size (-0.038 mm), the sample is fed into flotation. 150 g / t of calcium oxide, 60 g / t of water glass, and 2 g / t of MIBC are added as modifiers. The sample is then subjected to cleaning operation I to obtain cleaning concentrate I and cleaning middlings I. The cleaning middlings I are returned to the pulp conditioning process and fed into the roughing process. The cleaning concentrate I is then subjected to cleaning operation II. 10 g / t of calcium oxide, 30 g / t of water glass, and 5 g / t of MIBC are added as modifiers. The cleaning operation II yields cleaning concentrate II and cleaning middlings II. The cleaning middlings II are returned to the pulp conditioning process and fed into cleaning operation I. After one roughing, two cleaning, and three scavenging processes, the molybdenite concentrate is obtained.
[0043] (5) Add 75g / t of water glass, 20g / t of compound collector, and 10g / t of MIBC to the molybdenite tailings from step (1) in sequence, and perform scavenging operation I to obtain scavenging I middlings and scavenging I tailings. The scavenging I middlings are returned to the roughing operation. Add 100g / t of calcium oxide, 15g / t of water glass, 10g / t of compound collector, and 10g / t of MIBC to the scavenging I tailings, and perform scavenging operation II to obtain scavenging II middlings and scavenging II tailings. The scavenging II middlings are returned to the roughing operation. Add 15g / t of water glass, 4g / t of compound collector, and 5g / t of MIBC to the scavenging II tailings, and perform scavenging operation III to obtain scavenging III middlings and scavenging III tailings. The scavenging III middlings are returned to the roughing operation. The scavenging III tailings are the final tailings.
[0044] In this embodiment, the molybdenite concentrate has a molybdenum grade of 1.10% and a molybdenum recovery rate of 75.67%.
[0045] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made to it in form and detail without departing from the scope defined by the claims of the present invention.
Claims
1. A collector for fine-grained molybdenite, characterized in that, The collector is a compound hydrocarbon oil collector, comprising pyrolysis oil, 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2], and kerosene. This compound hydrocarbon oil collector is used to collect fine-grained molybdenite with high clay content and low grade. The preparation method of the compound hydrocarbon oil collector is as follows: The pyrolysis oil and 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt [AMIM][NTF2] were mixed in a mass ratio of 7:20 to 9:20 and then extracted with ultrasound for 1 hour. The mixture was then placed in a constant temperature water bath and allowed to stand for 2 hours. The extract was then collected and combined with kerosene in a mass ratio of 1:3 to form the compound hydrocarbon oil collector.
2. The application of the collector for fine-grained molybdenite according to claim 1 in the collection of high-muddy, low-grade fine-grained molybdenite, characterized in that, The flotation process employs a roughing, cleaning, and scavenging phase, as detailed below: The raw ore is ground to a particle size of less than 0.074 mm by mass, accounting for 60% to 65%. The slurry concentration is adjusted to 30% to 45%. Then, a modifier, the compound hydrocarbon oil collector, and a frother are added to the slurry for a roughing operation to obtain molybdenite roughing concentrate and molybdenite roughing tailings. After regrinding the molybdenite concentrate from step (1) to 90% of the -0.038mm, it is put into flotation. A modifier and a frother are added for two cleaning operations. The first cleaning operation yields the first cleaning concentrate and the second cleaning medium. The modifier and frother are added to the first cleaning concentrate for the second cleaning operation to obtain the molybdenite concentrate and the second cleaning medium. The second cleaning medium is returned to the first roughing operation, and the second cleaning medium is returned to the first cleaning operation to form a closed loop. Add the modifier, the compound hydrocarbon oil collector, and the frother to the molybdenite roughing tailings from step (1), and perform three scavenging operations. The middlings from the three scavenging operations are mixed and returned to the roughing operation to form a closed loop, thus obtaining the tailings.
3. The application of the collector for fine-grained molybdenite according to claim 2 in the collection of high-muddy, low-grade fine-grained molybdenite, characterized in that: The modifiers in steps (1) to (3) are calcium oxide and water glass, and the foaming agent is MIBC.
4. The application of the collector for fine-grained molybdenite according to claim 3 in the collection of high-muddy, low-grade fine-grained molybdenite, characterized in that: The dosages of the reagents in step (1) are as follows: 400-1000 g / t of calcium oxide modifier, 150-450 g / t of water glass, 60-80 g / t of compound hydrocarbon oil collector, and 48-60 g / t of MIBC foaming agent; the dosages of the reagents in step (2) are as follows: 100-200 g / t of calcium oxide modifier for Selective I, 15-80 g / t of water glass, and 0-10 g / t of MIBC foaming agent; 0-100 g / t of calcium oxide modifier for Selective II, 20-40 g / t of water glass, and 0-6 g / t of MIBC foaming agent; the dosages of the reagents in step (3) are as follows: 75-120 g / t of water glass for Scavenging I, 20-40 g / t of compound collector, and MIBC foaming agent. 10~40g / t, Scavenging II modifier calcium oxide 100~200g / t, water glass 15~80g / t, compound collector 10~25g / t, frother MIBC 10~20g / t, Scavenging III water glass 15~40g / t, compound collector 4~20g / t, frother MIBC 0~20g / t.
Citation Information
Patent Citations
Method for recycling titanium and iron in red mud through combination acid pickling and precipitate floatation
CN105219968A
Mo-MOF-based ion nanofluid as well as preparation method and application thereof
CN117625236A