A method for preparing titanium silicon molecular sieve

Through the preparation method of titanium-silicon molecular sieves, equipped with active nano-CoFe2O4 particles and surface treatment, the problem of treating phenolic organic pollutants in phenolic wastewater is solved, achieving efficient adsorption and degradation, avoiding secondary pollution, and improving treatment efficiency. and stability.

CN118598152BActive Publication Date: 2024-10-22ZHEJIANG TWRD NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088332.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing technology has secondary pollution problems when treating phenolic wastewater, and the Fenton method can only be performed under acidic conditions, making it difficult to effectively treat phenolic organic pollutants.

Method used

The preparation method of titanium silicon molecular sieve is adopted, and the active component - nanometer CoFe2O4 particles are carried through the sol-gel method, and 3-aminopropyltriethoxysilane is used for surface treatment to enhance the photocatalytic degradation and adsorption performance of titanium silicon molecular sieve. , to avoid secondary pollution.

Benefits of technology

It achieves efficient adsorption and degradation of phenolic organic pollutants in phenolic wastewater, improves treatment efficiency, and reduces the loss of titanium, iron, and cobalt ions during the long-term service of titanium-silicon molecular sieves, avoiding secondary damage to the water body. pollute.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of a titanium silicon molecular sieve, belonging to the technical field of molecular sieves. The preparation method comprises the following steps: tetraethyl silicate, deionized water, tetrapropylammonium hydroxide, tetraethyl titanate and isopropyl alcohol are mixed and stirred according to a molar ratio of SiO2:H2O:tetrapropylammonium hydroxide:TiO2:isopropyl alcohol=1:15-22:0.25-0.35:0.025-0.035:4.4-4.5, and then subjected to post-treatment such as roasting to obtain a carrier, and then active component-nano CoFe2O4 particles are carried on the surface of the carrier by a sol-gel method, and then 3-aminopropyltriethoxysilane is used for surface treatment to obtain a titanium silicon molecular sieve for treating phenol-containing wastewater. The titanium silicon molecular sieve prepared by the invention realizes efficient treatment of phenolic organic pollutants in the phenol-containing wastewater by photocatalytic degradation and adsorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of molecular sieves, and in particular relates to a method for preparing a titanium silicon molecular sieve. Background Art

[0002] The output of coal chemical wastewater is huge, which contains a large amount of harmful substances, especially phenol-containing wastewater.

[0003] Phenolic wastewater refers to wastewater containing phenolic compounds such as phenol, cresol, o-xylene, and catechol. Phenolic wastewater usually comes from the discharge of gas purification, desulfurization, gas conversion and other processes. Phenolic wastewater is highly toxic, irritating and difficult to handle. If it is left unchecked and discharged directly, it will cause great harm to the environment, humans and animals.

[0004] At present, there are three main types of treatment processes for phenol-containing wastewater, namely physical treatment, biochemical treatment and chemical oxidation. Among them, the Fenton method in the chemical oxidation method is widely used in phenol-containing wastewater due to its strong oxidizing property, fast oxidation rate and high quantization efficiency. The Fenton method mainly utilizes the activation effect of Fe, and the reaction process is efficient and the process is simple. However, the Fenton method can only be carried out under acidic conditions, and the added iron ions are prone to cause secondary pollution of the water body. Therefore, the present application focuses on titanium silicon molecular sieves that also have an activation effect.

[0005] Titanium silicon molecular sieve is a heteroatom molecular sieve with the advantages of strong adsorption, good acid resistance, excellent selective catalytic oxidation performance, etc., and is widely used in various catalytic oxidation reactions in industry. Among them, since the skeleton titanium atoms in the titanium silicon molecular sieve exist in a tetracoordinated form, they form a titanium oxide tetrahedron structure with high energy with oxygen atoms, and have the potential to accept electron pairs and transform into hexacoordinated titanium, so they have the ability to adsorb and activate H2O2, and are often used in the fields of cyclohexanone oximation, phenol hydroxylation, alkane oxidation, olefin epoxidation, etc. Based on this, the present invention aims to develop the application of titanium silicon molecular sieve in phenol-containing wastewater, prevent secondary pollution to phenol-containing wastewater, and improve the adsorption / degradation of phenolic organic pollutants in phenol-containing wastewater. Summary of the invention

[0006] The present invention aims to develop the application of titanium silicate molecular sieve in phenol-containing wastewater, prevent secondary pollution of the phenol-containing wastewater, and improve the adsorption / degradation of phenolic organic pollutants in the phenol-containing wastewater. To this end, the present invention provides a preparation method of titanium silicate molecular sieve.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for preparing a titanium silicon molecular sieve comprises the following steps:

[0009] S1. Mix tetraethyl silicate, deionized water and tetrapropylammonium hydroxide, fill with nitrogen for protection, and then add tetraethyl titanate and isopropyl alcohol, the molar ratio of each raw material is SiO2:H2O:tetrapropylammonium hydroxide:TiO2:isopropyl alcohol=1:15-22:0.25-0.35:0.025-0.035:4.4-4.5. After the addition is completed, stir for 4-5 hours. After the stirring is completed, a mixed component is obtained, and the mixed component is further post-treated to obtain a carrier;

[0010] S2, adding a carrier to the active solution with stirring to obtain a suspension, and the suspension is stirred, dried and calcined to obtain a calcined powder;

[0011] S3. Add the calcined powder and 3-aminopropyltriethoxysilane to anhydrous ethanol with stirring, stir at room temperature for 2 to 3 hours, filter, wash the filter cake with deionized water for 3 to 5 times, and finally dry at 60° C. for 12 hours, cool to room temperature, and obtain titanium silicalite.

[0012] Furthermore, the molar ratio of the raw materials described in S1 is SiO2:H2O:tetrapropylammonium hydroxide:TiO2:isopropanol=1:20:0.3:0.03:4.5.

[0013] Furthermore, the post-processing in S1 includes the following steps:

[0014] The mixed components were heated to 80°C to remove alcohol for 1 hour, and deionized water of the same volume as the dealcohol was added. After the addition was completed, the temperature was raised to 155-160°C and crystallized for 48 hours. After the crystallization was completed, it was cooled to room temperature and centrifuged to take the solid component. The solid component was washed three times with deionized water, then placed in a 100°C drying oven to constant weight, and then placed in a muffle furnace at 500°C for 6 hours. After the calcination was completed, it was cooled to room temperature to obtain a carrier.

[0015] Furthermore, the usage ratio of the carrier and the active liquid in S2 is 1 g:5 mL.

[0016] Further, the stirring, drying and roasting process in S2 comprises the following steps:

[0017] The suspension is heated to 55-60°C and stirred at a constant temperature for 2-3 hours to obtain a sol-like component. The sol-like component is placed in a constant temperature drying oven at 80-90°C and dried at a constant temperature for 5-6 hours to obtain a precursor. The precursor is placed in a muffle furnace and calcined at 550°C for 2 hours. After calcination, a calcined powder is obtained.

[0018] Furthermore, the dosage ratio of the anhydrous ethanol, the calcined powder and the auxiliary agent in S3 is 100 mL: 4.5-5.0 g: 2.5-4.0 g.

[0019] Furthermore, the active solution in S2 is prepared by the following steps:

[0020] Add cobalt nitrate hexahydrate and ferric nitrate nonahydrate to ultrapure water, stir and mix evenly to obtain a mixed solution, and then place the mixed solution in a 50-60°C water bath and stir at a constant temperature for 2-3 hours. After completion, add citric acid thereto and stir, continue to stir at a constant temperature for 1-2 hours, and after completion, cool to room temperature to obtain an active solution.

[0021] Furthermore, the usage ratio of the ultrapure water, cobalt nitrate hexahydrate and ferric nitrate nonahydrate is 200 mL: 14.5 g: 40.4 g.

[0022] Furthermore, the molar concentration of the citric acid is equal to the sum of the molar concentrations of the metal ions in the mixed solution.

[0023] Beneficial effects of the present invention:

[0024] The present invention carries active components - nano CoFe2O4 particles on the surface of an existing titanium silicalite by a sol-gel method, and then uses 3-aminopropyltriethoxysilane for surface treatment to obtain a titanium silicalite for treating phenol-containing wastewater. The titanium silicalite prepared by the present invention uses photocatalytic degradation and adsorption to achieve efficient treatment of phenolic organic pollutants in phenol-containing wastewater. The specific principle is as follows:

[0025] Firstly, the interior of the titanium silicalite molecular sieve has an -O-Ti-O-semiconductor chain, which can be excited by ultraviolet rays and has photocatalytic oxidation performance. The present invention provides an application of a titanium silicalite molecular sieve in the field of photocatalytic degradation of wastewater, and through experiments, the titanium silicalite molecular sieve prepared by the preparation method of the present invention has excellent adsorption / degradation effect on phenol-containing wastewater.

[0026] Secondly, the cobalt ions and iron ions in the active component-nano CoFe2O4 particles have excellent photocatalytic activity. Among them, Fe2O3 formed by iron ions can effectively degrade organic pollutants in water under visible light irradiation, and the present invention further improves its photocatalytic degradation performance by doping Co. Finally, the present invention carries the active component-nano CoFe2O4 particles on the carrier surface through a sol-gel method, and finally improves the photocatalytic degradation performance of the prepared titanium silicon molecular sieve.

[0027] Then, the carrier prepared by the present invention has a three-dimensional pore structure (intrinsic structure of titanium silicalite molecular sieve), has a large specific surface area and excellent adsorption performance, can adsorb phenolic organic pollutants in phenol-containing wastewater into the pores and surfaces through adsorption, forming a local high-concentration treatment environment, and then undergoes photocatalytic degradation, active free radicals generated on the surface of the titanium silicalite molecular sieve preferentially react with phenolic organic pollutants adsorbed in the pores, the organic pollutants are degraded, the reaction products are desorbed into the solution, and the adsorption performance of the titanium silicalite molecular sieve is regenerated. At the same time, the nano CoFe2O4 particles loaded on the inner and outer surfaces of the titanium silicalite pores can improve the degradation efficiency of the organic pollutants, further improving the degradation efficiency.

[0028] Next, the 3-aminopropyltriethoxysilane of the present invention is subjected to surface treatment, and the hydrolysis of the silicon-oxygen bond in the 3-aminopropyltriethoxysilane is utilized to enhance the wettability and dispersibility of the titanium silicon molecular sieve. At the same time, the 3-aminopropyltriethoxysilane contains amino groups, which can interact with phenolic organic pollutants in phenolic wastewater through hydrogen bonds, thereby improving the adsorption of phenolic organic pollutants by the titanium silicon molecular sieve. In addition, the amino groups can chelate with the titanium ions, iron ions and cobalt ions in the titanium silicon molecular sieve through coordination, thereby helping to reduce the secondary pollution of the phenolic wastewater caused by the loss of titanium ions, iron ions and cobalt ions during the long-term service of the titanium silicon molecular sieve. At the same time, the presence of chelation helps to improve the stability and durability of the adsorption / degradation of the titanium silicon molecular sieve.

[0029] Finally, the nano CoFe2O4 particles are magnetic. The present invention introduces them into the preparation of titanium silicon molecular sieve, which helps to improve the separation efficiency of titanium silicon molecular sieve, helps to reduce or even eliminate the secondary pollution of water bodies caused by titanium silicon molecular sieve, and also improves the treatment process of phenol-containing wastewater and the recovery rate of titanium silicon molecular sieve. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] Preparation of active solution:

[0033] To 200 mL of ultrapure water, 14.5 g (0.05 mol) of cobalt nitrate hexahydrate (99%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) and 40.4 g (0.1 mol) of ferric nitrate nonahydrate (99.99%; purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added, that is, the molar ratio of cobalt ions to iron ions was controlled to be 1:2, and the mixture was stirred and mixed evenly to obtain a mixed solution. The mixed solution was then placed in a 50°C water bath and stirred at a constant temperature for 2 hours. After completion, citric acid (99.5%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added thereto with stirring, and the molar concentration of citric acid was controlled to be equal to the sum of the molar concentrations of metal ions in the mixed solution. After the addition of citric acid, the mixture was stirred at a constant temperature for 1 hour. After completion, the mixture was cooled to room temperature to obtain an active solution.

[0034] Example 2

[0035] Preparation of active solution:

[0036] To 200 mL of ultrapure water, 14.5 g (0.05 mol) of cobalt nitrate hexahydrate (99%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) and 40.4 g (0.1 mol) of ferric nitrate nonahydrate (99.99%; purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added, that is, the molar ratio of cobalt ions to iron ions was controlled to be 1:2, and the mixture was stirred and mixed evenly to obtain a mixed solution. The mixed solution was then placed in a 55°C water bath and stirred at a constant temperature for 3 hours. After completion, citric acid (99.5%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added thereto with stirring, and the molar concentration of citric acid was controlled to be equal to the sum of the molar concentrations of metal ions in the mixed solution. After the addition of citric acid, the mixture was stirred at a constant temperature for 2 hours. After completion, the mixture was cooled to room temperature to obtain an active solution.

[0037] Example 3

[0038] Preparation of active solution:

[0039] To 200 mL of ultrapure water, 14.5 g (0.05 mol) of cobalt nitrate hexahydrate (99%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) and 40.4 g (0.1 mol) of ferric nitrate nonahydrate (99.99%; purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added, that is, the molar ratio of cobalt ions to iron ions was controlled to be 1:2, and the mixture was stirred and mixed evenly to obtain a mixed solution. The mixed solution was then placed in a 60°C water bath and stirred at a constant temperature for 3 hours. After completion, citric acid (99.5%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added thereto with stirring, and the molar concentration of citric acid was controlled to be equal to the sum of the molar concentrations of metal ions in the mixed solution. After the addition of citric acid, the mixture was stirred at a constant temperature for 2 hours. After completion, the mixture was cooled to room temperature to obtain an active solution.

[0040] Example 4

[0041] A method for preparing a titanium silicon molecular sieve comprises the following steps:

[0042] S1. Tetraethyl silicate (TEOS, 99.99% purity, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), deionized water (homemade) and tetrapropylammonium hydroxide (TPAOH, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added to the reactor, stirred for 30 minutes, filled with nitrogen for protection, and then tetraethyl titanate (TBOT, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and isopropyl alcohol (IPA, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added thereto, wherein the molar ratio of each raw material is SiO 2: H2O: tetrapropylammonium hydroxide: TiO2: isopropanol = 1:15:0.25:0.025:4.4. After the addition is completed, stir for 4 hours. After the stirring is completed, heat it to 80°C to remove alcohol for 1 hour, and add deionized water with the same volume as the dealcohol. After the addition is completed, heat it to 155°C and crystallize for 48 hours. After the crystallization is completed, cool it to room temperature, centrifuge it, take the solid component, wash the solid component three times with deionized water, and then place it in a 100°C drying oven to dry to constant weight, and then place it in a muffle furnace at 500°C for 6 hours. After the calcination is completed, cool it to room temperature to obtain a carrier;

[0043] S2. Add the carrier to the active solution prepared in Example 1 at a solid-liquid ratio of 1 g: 5 mL with stirring, heat the system to 55° C., and stir at a constant temperature for 2 h to obtain a sol-like component, place the sol-like component in a constant temperature drying oven at 80° C. and dry at a constant temperature for 5 h to obtain a precursor, place the precursor in a muffle furnace at 550° C. and calcine for 2 h to obtain a calcined powder after calcination;

[0044] S3. Add 4.5 g of the calcined powder and 2.5 g of 3-aminopropyltriethoxysilane (99%, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) into 100 mL of anhydrous ethanol with stirring, stir at room temperature for 2 h, filter, wash the filter cake with deionized water 3 times, and finally dry at 60°C for 12 h, cool to room temperature, and obtain titanium silicalite molecular sieve.

[0045] Example 5

[0046] A method for preparing a titanium silicon molecular sieve comprises the following steps:

[0047] S1. Tetraethyl silicate (TEOS, 99.99% purity, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), deionized water (homemade) and tetrapropylammonium hydroxide (TPAOH, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added to the reactor, stirred for 30 minutes, filled with nitrogen for protection, and then tetraethyl titanate (TBOT, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and isopropyl alcohol (IPA, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added thereto, wherein the molar ratio of each raw material was Si: O2:H2O:tetrapropylammonium hydroxide:TiO2:isopropanol=1:20:0.3:0.03:4.5. After the addition is completed, stir for 5 hours. After the stirring is completed, heat it to 80℃ to remove alcohol for 1 hour, and add deionized water with the same volume as the dealcohol. After the addition is completed, heat it to 160℃ and crystallize for 48 hours. After the crystallization is completed, cool it to room temperature, centrifuge it, take the solid component, wash the solid component three times with deionized water, dry it in a 100℃ drying oven to constant weight, and then place it in a muffle furnace at 500℃ for 6 hours. After the calcination is completed, cool it to room temperature to obtain a carrier;

[0048] S2. Add the carrier to the active solution prepared in Example 2 at a solid-liquid ratio of 1g:5mL with stirring, heat the system to 58°C, and stir at a constant temperature for 3h to obtain a sol-like component, place the sol-like component in a constant temperature drying oven at 85°C and dry at a constant temperature for 6h to obtain a precursor, place the precursor in a muffle furnace at 550°C and calcine for 2h, and after calcination, obtain a calcined powder;

[0049] S3. Add 5 g of the calcined powder and 4 g of 3-aminopropyltriethoxysilane (99%, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) into 100 mL of anhydrous ethanol with stirring, stir at room temperature for 3 h, filter, wash the filter cake with deionized water 5 times, and finally dry at 60°C for 12 h, cool to room temperature, and obtain titanium silicalite molecular sieve.

[0050] Example 6

[0051] A method for preparing a titanium silicon molecular sieve comprises the following steps:

[0052] S1. Tetraethyl silicate (TEOS, 99.99% purity, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), deionized water (homemade) and tetrapropylammonium hydroxide (TPAOH, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added to the reactor, stirred for 30 minutes, filled with nitrogen for protection, and then tetraethyl titanate (TBOT, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and isopropyl alcohol (IPA, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added thereto, wherein the molar ratio of each raw material is SiO 2: H2O: tetrapropylammonium hydroxide: TiO2: isopropanol = 1:22:0.35:0.035:4.5. After the addition is completed, stir for 5 hours. After the stirring is completed, heat it to 80°C to remove alcohol for 1 hour, and add deionized water with the same volume as the dealcohol. After the addition is completed, heat it to 160°C and crystallize for 48 hours. After the crystallization is completed, cool it to room temperature, centrifuge it, take the solid component, wash the solid component three times with deionized water, and then place it in a 100°C drying oven to dry to constant weight, and then place it in a muffle furnace at 500°C for 6 hours. After the calcination is completed, cool it to room temperature to obtain a carrier;

[0053] S2. Add the carrier to the active solution prepared in Example 3 at a solid-liquid ratio of 1g:5mL with stirring, heat the system to 60°C, and stir at a constant temperature for 3h to obtain a sol-like component, place the sol-like component in a constant temperature drying oven at 90°C and dry at a constant temperature for 6h to obtain a precursor, place the precursor in a muffle furnace at 550°C and calcine for 2h, and after calcination, obtain a calcined powder;

[0054] S3. Add 5.0 g of the calcined powder and 4.0 g of 3-aminopropyltriethoxysilane (99%, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) to 100 mL of anhydrous ethanol with stirring, stir at room temperature for 3 h, filter, wash the filter cake with deionized water 5 times, and finally dry at 60°C for 12 h, cool to room temperature, and obtain titanium silicalite molecular sieve.

[0055] Comparative Example 1

[0056] Comparative Example 1 is the control group of Example 5, and steps S2 and S3 in Example 5 are removed, that is, the active component loading and surface treatment process are removed, as follows:

[0057] A method for preparing a titanium silicon molecular sieve comprises the following steps:

[0058] Tetraethyl silicate (TEOS, 99.99% purity, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), deionized water (homemade) and tetrapropylammonium hydroxide (TPAOH, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added to the reactor, stirred for 30 minutes, filled with nitrogen for protection, and then tetraethyl titanate (TBOT, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and isopropyl alcohol (IPA, analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were added thereto, wherein the molar ratio of each raw material was SiO2: H2O:tetrapropylammonium hydroxide:TiO2:isopropanol=1:20:0.3:0.03:4.5. After adding, stir for 5 hours. After stirring, heat to 80℃ to remove alcohol for 1 hour, and add deionized water with the same volume as the dealcohol. After adding, heat to 160℃ and crystallize for 48 hours. After crystallization, cool to room temperature, centrifuge, take solid components, wash the solid components three times with deionized water, dry them in a 100℃ drying oven to constant weight, and then place them in a muffle furnace at 500℃ for calcination for 6 hours. After calcination, cool to room temperature to obtain titanium silicon molecular sieve.

[0059] Comparative Example 2

[0060] Commercially available titanium silicate molecular sieve (TS-1; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.).

[0061] Test Example 1

[0062] The titanium silicon molecular sieves prepared in Examples 4 to 6 and Comparative Examples 1 to 2 were subjected to treatment of phenol-containing wastewater. The treatment process is as follows. The treatment results are shown in Table 1:

[0063] First, the phenol-containing wastewater comes from a coal chemical plant in Zhejiang. The main components and contents of the phenol-containing wastewater from the coal chemical plant are shown in Table 1 below:

[0064] Table 1 Main components and contents of phenolic wastewater from coal chemical plants

[0065] project Monophenol content (mg / L) Polyphenol content (mg / L) Total phenol content (mg / L) Total ammonia (mg / L) COD content (mg / L) content 3000~5000 2000~4000 5000~9000 4000~10000 15000~20000

[0066] After the above phenol-containing wastewater is pretreated in the coal chemical plant (anaerobic + aerobic biological treatment), the main components and contents of the pretreated phenol-containing wastewater are shown in Table 2 below:

[0067] Table 2 Main components and contents of phenol-containing wastewater after pretreatment

[0068] project Monophenol content (mg / L) Polyphenol content (mg / L) Total phenol content (mg / L) Total ammonia (mg / L) COD content (mg / L) content 370~550 250~350 620~900 220~500 270~400

[0069] Then, this test example conducted a degradation test of titanium silicalite on the above-mentioned pretreated phenol-containing wastewater. A total of 100L of pretreated phenol-containing wastewater was taken as the wastewater to be tested, and the composition and content of the wastewater to be tested were specifically detected, as shown in Table 3 below:

[0070] Table 3 Main components and contents of wastewater to be tested

[0071] project Monophenol content (mg / L) Polyphenol content (mg / L) Total phenol content (mg / L) Total ammonia (mg / L) COD content (mg / L) content 485 278 763 325 310

[0072] Next, the wastewater to be tested was divided into several parts, and the degradation test of the wastewater to be tested was carried out using the titanium silicon molecular sieve prepared in the embodiment / comparative example. The test conditions were divided into ultraviolet light / sunlight / dark conditions. The ultraviolet light conditions used an ultraviolet germicidal lamp (20W) produced by Guangzhou Langpu Optoelectronics Technology Co., Ltd., and 2g of the titanium silicon molecular sieve prepared in the embodiment / comparative example was stirred into the wastewater to be tested. After stirring for 1h at a stirring rate of 100r / min, the titanium silicon molecular sieve was filtered to remove the titanium silicon molecular sieve, and then the composition and content of the remaining wastewater to be tested were detected. Three tests were carried out under ultraviolet light / sunlight / dark conditions for each group of embodiments / comparative examples, and the average value was finally taken. The test results are shown in Table 4 below:

[0073] Table 4 Test results of wastewater degradation

[0074]

[0075] It can be seen from Table 4 that the titanium silicate molecular sieves prepared in Examples 4 to 6 of the present invention have excellent adsorption / degradation effects on phenolic organic pollutants in phenol-containing wastewater.

[0076] It should be noted that, in this article, terms such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or equipment that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment.

[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing titanium silicon molecular sieve, It is characterized in that The following steps are involved: S1. Tetraethyl silicate, deionized water and tetrapropylammonium hydroxide are mixed and stirred, and nitrogen is introduced for protection. Then tetraethyl titanate and isopropanol are added thereto. The molar ratio of each raw material is SiO 2 :H 2 O:Tetrapropylammonium hydroxide:TiO 2 : isopropanol = 1: 15-22: 0.25-0.35: 0.025-0.035: 4.4-4.

5. After the addition is completed, stir for 4-5 hours. After the stirring is completed, a mixed component is obtained. The mixed component is then post-treated to obtain a carrier; S2, adding a carrier to the active solution with stirring to obtain a suspension, and the suspension is stirred, dried and calcined to obtain a calcined powder; S3, adding the calcined powder and 3-aminopropyltriethoxysilane to anhydrous ethanol with stirring, stirring at room temperature for 2-3 hours, filtering, washing the filter cake with deionized water for 3-5 times, and finally drying at 60° C. for 12 hours, cooling to room temperature, and obtaining a titanium silicon molecular sieve; The active solution in S2 is prepared by the following steps: Add cobalt nitrate hexahydrate and ferric nitrate nonahydrate to ultrapure water, stir and mix evenly to obtain a mixed solution, and then place the mixed solution in a 50-60°C water bath and stir at a constant temperature for 2-3 hours. After completion, add citric acid thereto and stir, continue to stir at a constant temperature for 1-2 hours, and after completion, cool to room temperature to obtain an active solution.

2. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The molar ratio of the raw materials described in S1 is SiO 2 :H 2 O:Tetrapropylammonium hydroxide:TiO 2 :isopropyl alcohol=1:20:0.3:0.03:4.

5.

3. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The post-processing described in S1 includes the following steps: The mixed components were heated to 80°C to remove alcohol for 1 hour, and deionized water of the same volume as the dealcohol was added. After the addition was completed, the temperature was raised to 155-160°C and crystallized for 48 hours. After the crystallization was completed, it was cooled to room temperature and centrifuged to take the solid component. The solid component was washed three times with deionized water, then placed in a 100°C drying oven to constant weight, and then placed in a muffle furnace at 500°C for 6 hours. After the calcination was completed, it was cooled to room temperature to obtain a carrier.

4. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The usage ratio of the carrier and the active liquid in S2 is 1 g:5 mL.

5. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The stirring, drying and roasting process described in S2 comprises the following steps: The suspension is heated to 55-60°C and stirred at a constant temperature for 2-3 hours to obtain a sol-like component. The sol-like component is placed in a constant temperature drying oven at 80-90°C and dried at a constant temperature for 5-6 hours to obtain a precursor. The precursor is placed in a muffle furnace and calcined at 550°C for 2 hours. After calcination, a calcined powder is obtained.

6. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The usage ratio of anhydrous ethanol, calcined powder and auxiliary agent in S3 is 100mL:4.5-5.0g:2.5-4.0g.

7. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The usage ratio of the ultrapure water, cobalt nitrate hexahydrate and ferric nitrate nonahydrate is 200 mL: 14.5 g: 40.4 g.

8. The method for preparing a titanium silicon molecular sieve according to claim 1, It is characterized in that The molar concentration of the citric acid is equal to the sum of the molar concentrations of the metal ions in the mixed solution.