A method and system for treating fluorine-containing sludge

CN118598447BActive Publication Date: 2024-11-12ZHEJIANG WATER HEALER ENVIRONMENTAL TECH CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202411045498.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

目前针对含氟光伏废水普遍采用化学/混凝沉淀、浮选、吸附等方法处理,处理后会产生大量含氟污泥,含氟污泥的主要成分为CaF2、SiO2、CaSO4、Ca(OH)2、沉淀剂和絮凝剂等,造成了后续处理难的问题

Benefits of technology

[0051] The invention uses fluorine-containing sludge waste in the photovoltaic and photoelectric industry as raw material. After treating the fluorine-containing sludge, it can efficiently convert calcium fluoride into HF products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118598447B_ABST
    Figure CN118598447B_ABST
Patent Text Reader

Abstract

The present invention provides a method and system for treating fluorine-containing sludge, and belongs to the technical field of fluorine-containing sludge treatment. The method for treating fluorine-containing sludge of the present invention uses fluorine-containing sludge waste in the photovoltaic industry as raw material, extracts and separates calcium fluoride and calcium salt in the fluorine-containing sludge through impurity removal treatment and first acidification treatment, converts calcium fluoride into crude HF through second acidification treatment, removes impurities from the crude HF through oxidation treatment and distillation treatment, obtains HF liquid with high yield, and realizes resource utilization of fluorine-containing sludge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorine-containing sludge treatment, and in particular to a method and system for treating fluorine-containing sludge. Background Art

[0002] In recent years, my country has vigorously supported the new energy industry, information technology has developed rapidly, and the photovoltaic industry has developed rapidly, accounting for more than 50% of the global market share. In the process of cleaning and etching photovoltaic glass and silicon wafers, the photovoltaic industry uses a large amount of hydrofluoric acid to corrode silicon materials, thereby discharging fluorine-containing wastewater. At present, chemical / coagulation sedimentation, flotation, adsorption and other methods are generally used to treat fluorine-containing photovoltaic wastewater. After treatment, a large amount of fluorine-containing sludge will be produced. The main components of fluorine-containing sludge are CaF2, SiO2, CaSO4, Ca(OH)2, precipitants and flocculants, etc., which makes subsequent treatment difficult.

[0003] The traditional disposal method of fluoride-containing sludge is direct landfill treatment. Its advantages are simplicity and convenience, but its disadvantages are waste of resources and occupation of land. Moreover, as the landfill time increases, fluoride ions will leach into the environment and cause fluoride pollution, which also wastes precious fluorine resources.

[0004] The main component of fluorine-containing sludge is CaF2. Proper disposal and efficient conversion of it can not only eliminate the potential pollution of fluorine-containing sludge, but also find a substitute for non-renewable fluorite resources. Summary of the invention

[0005] The invention provides a method for treating fluorine-containing sludge, which can realize resource utilization of fluorine-containing sludge.

[0006] The present invention also provides a system for executing the above treatment method, and each reactor is reasonably connected to achieve the treatment of fluorine-containing sludge.

[0007] The first aspect of the present invention provides a method for treating fluorine-containing sludge, which comprises the following steps:

[0008] 1) mixing the fluorine-containing sludge, carbonate solution and dispersant to perform impurity removal treatment, and obtaining impurity-removed fluorine-containing sludge when the pH value is 7-7.5;

[0009] 2) subjecting the impurity-removed fluorine-containing sludge to a first acidification treatment with a hydrofluoric acid solution to obtain a crude calcium fluoride product;

[0010] 3) subjecting the crude calcium fluoride to a second acidification treatment with sulfuric acid to obtain a crude HF product and calcium sulfate; the sulfuric acid comprises 98% sulfuric acid and 20% oleum;

[0011] 4) oxidizing the crude HF product with fluorine gas to obtain a gas phase product;

[0012] 5) The gas phase product is subjected to rectification treatment to obtain refined HF and light impurity gas phase.

[0013] The method as described above, wherein before step 5), further comprises:

[0014] Performing a first condensation treatment on the gas phase product to obtain a condensate product;

[0015] returning part of the condensate product to participate in the oxidation treatment, and subjecting the remaining part of the condensate product to the refining treatment;

[0016] The volume ratio of the condensate product returned to participate in the oxidation treatment to the condensate product subjected to the refining treatment is 3-7.

[0017] The method as described above, wherein the second acidification treatment comprises:

[0018] pretreating the crude calcium fluoride and mixing it with sulfuric acid to obtain a solid-liquid mixture;

[0019] Performing acidification pretreatment on the solid-liquid mixture to obtain an acidified gas phase product and an acidified solid-liquid mixture;

[0020] The acidified solid-liquid mixture is subjected to acidification intermediate treatment and acidification post-treatment in sequence to obtain a first HF crude product;

[0021] The acidified gas phase product is fractionated to obtain a second HF crude product and an acidic heavy component;

[0022] Wherein, the HF crude product in step 4) includes a first HF crude product and a second HF crude product;

[0023] The temperature of the pretreatment is 150-200°C, the temperature of mixing with sulfuric acid is 50-60°C, the temperature of the acidification pre-treatment is 80-120°C, the temperature of the acidification treatment is 180-300°C, and the temperature of the acidification post-treatment is 150-200°C.

[0024] The method as described above, wherein, after the acidic heavy component is purified, the purified product is used as the hydrofluoric acid solution to participate in the first acidification treatment;

[0025] and / or; performing a second condensation treatment on the light impurity gas phase in step 5) to obtain a liquid phase product and gas phase impurities;

[0026] The liquid phase impurities are returned to participate in the distillation process; the volume ratio of the liquid phase product to the gas phase impurities is 2-5;

[0027] The gas phase impurities are absorbed by an absorbent to obtain by-products of calcium fluorosilicate and calcium sulfate.

[0028] The method as described above, wherein the temperature of the impurity removal treatment in step 1) is 40-60°C;

[0029] And / or, the carbonate solution in step 1) includes at least one of a Na2CO3 solution and a K2CO3 solution;

[0030] and / or, in step 1), the dispersant comprises at least one of polyethylene glycol and polysorbate;

[0031] and / or, step) 2: the temperature of the first acidification treatment is 20-35°C;

[0032] And / or, the volume ratio of 98% sulfuric acid to 20% oleum in step) 3 is 1.5-2;

[0033] And / or, the mass ratio of the crude calcium fluoride product to the acidic solvent in step) 3 is 1 to 1.4;

[0034] And / or, the temperature of the oxidation treatment in step) 4 is 20-35°C;

[0035] And / or, the temperature of the first condensation treatment is 15-25°C;

[0036] And / or, the temperature of the second condensation treatment is 10-15°C.

[0037] A second aspect of the present invention provides a system for performing the above method, which comprises an alkalization reactor, a first acidification reactor, a second acidification reactor, an oxidation tower and a distillation tower;

[0038] The outlet of the alkalization reactor is connected to the inlet of the first acidification reactor, the outlet of the first acidification reactor is connected to the inlet of the second acidification reactor, the gas phase outlet of the second acidification reactor is connected to the gas inlet of the oxidation tower, and the gas phase outlet of the oxidation tower is connected to the inlet of the distillation tower.

[0039] The system as described above, wherein it further comprises a first condenser, and the oxidation tower and the distillation tower are connected via the first condenser;

[0040] The gas phase outlet of the oxidation tower is located above the oxidation tower, the gas phase outlet of the first condenser is connected to the inlet of the distillation tower, and the liquid phase outlet of the first condenser is connected to the upper inlet of the oxidation tower.

[0041] The system as described above, wherein the second acidification reactor comprises a pre-reactor and a rotary reactor which are interconnected, the pre-reactor and the rotary reactor are detachably connected, the outlet of the first acidification reactor is connected to the inlet of the pre-reactor, and the gas phase outlet of the rotary reactor is connected to the inlet of the oxidation tower;

[0042] A scraper is provided on the rotating shaft of the pre-reactor, and the rotation directions of the scraper and the pre-reactor are opposite;

[0043] A slag return cylinder is arranged on the rotating shaft of the rotary reactor, and the rotation direction of the slag return cylinder and the rotary reactor are opposite, and a material lifting member and a material blocking member bent in the opposite direction to the inlet of the pre-reactor are arranged on the inner wall of the rotary reactor;

[0044] The rotary reaction furnace is provided with electric heating devices at the furnace head and furnace tail respectively;

[0045] And / or, it also includes a distillation tower, the gas phase outlet of the pre-reactor is connected to the inlet of the distillation tower, and the gas phase outlet of the distillation tower is connected to the inlet of the oxidation tower.

[0046] The system as described above, wherein it further comprises a distiller, wherein the liquid phase outlet of the fractionation tower is communicated with the inlet of the distiller, and the gas phase outlet of the distiller is communicated with the inlet of the first acidification reactor.

[0047] The system as described above, wherein it further comprises a second condenser, the distillation product outlet of the distillation tower is connected to the inlet of the second condenser, the liquid product outlet of the second condenser is connected to the inlet of the distillation tower, and the gas product outlet of the second condenser is connected to the gas impurity treatment device;

[0048] And / or, a reboiling tray is arranged at the bottom of the oxidation tower, and the reboiling tray is located below the gas inlet of the oxidation tower;

[0049] And / or, the oxidation tower is provided with a gas inlet and a gas distributor at the bottom, the oxidation tower is provided with a liquid inlet and a liquid distributor at the top, and a packing layer is provided between the gas distributor and the liquid distributor;

[0050] And / or, a liquid storage tank is provided at the bottom of the distillation tower, and the temperature of the liquid storage tank is 18-30°C.

[0051] The present invention uses fluorine-containing sludge waste in the photovoltaic and photoelectric industries as raw materials, and after treating the fluorine-containing sludge, calcium fluoride can be efficiently converted into HF products. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0053] Figure 1A schematic diagram of a system provided in one embodiment of the present invention;

[0054] Figure 2 A schematic diagram of a system provided in one embodiment of the present invention;

[0055] Figure 3 is a schematic diagram of a second acidification reactor provided in one embodiment of the present invention;

[0056] Figure 4 A schematic diagram of an oxidation tower provided in one embodiment of the present invention;

[0057] Figure 5 It is a schematic diagram of a distillation tower provided in one embodiment of the present invention.

[0058] Description of reference numerals:

[0059] 1- alkalization reactor;

[0060] 2-first acidification reactor;

[0061] 3-second acidification reactor;

[0062] 301-pre-reactor;

[0063] 302-feeding port;

[0064] 303-acid import;

[0065] 304-scraping piece;

[0066] 305-pre-reactor gas phase outlet;

[0067] 306- spiral connection port;

[0068] 307- Rotary reactor;

[0069] 308-gas phase outlet of rotary reactor;

[0070] 309-slag return tube;

[0071] 310-Lifting parts;

[0072] 311- material stopper;

[0073] 312-slag outlet;

[0074] 4- Oxidation tower;

[0075] 401-air inlet;

[0076] 402- reboiling plate;

[0077] 403-Liquid distributor;

[0078] 404-gas distributor;

[0079] 405-circulation tank;

[0080] 406-Fluorine gas inlet;

[0081] 407-gas phase outlet;

[0082] 408-liquid inlet;

[0083] 409-filling layer;

[0084] 410-reboiler;

[0085] 5-Distillation tower;

[0086] 501-liquid storage tank;

[0087] 6- first condenser;

[0088] 7- fractionation tower;

[0089] 8- Distiller;

[0090] 9- Second condenser;

[0091] 10-Fluorine gas generator. DETAILED DESCRIPTION

[0092] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0093] The first aspect of the present invention provides a method for treating fluorine-containing sludge, comprising the following steps:

[0094] 1) mixing the fluorine-containing sludge, carbonate solution and dispersant to perform impurity removal treatment, and obtaining impurity-removed fluorine-containing sludge when the pH value is 7-7.5;

[0095] 2) subjecting the impurity-removed fluorine-containing sludge to a first acidification treatment with a hydrofluoric acid solution to obtain a crude calcium fluoride product;

[0096] 3) subjecting the crude calcium fluoride to a second acidification treatment with an acidic solvent to obtain a crude HF product and calcium sulfate; the acidic solvent comprises 98% sulfuric acid and 20% oleum;

[0097] 4) oxidizing the crude HF product with fluorine gas to obtain a gas phase product;

[0098] 5) The gas phase product is subjected to rectification treatment to obtain refined HF and light impurity gas phase.

[0099] The main components of the fluorine-containing sludge of the present invention are CaF2, SiO2, CaSO4, Ca(OH)2, precipitant and flocculant, etc. The addition of carbonate solution in step 1) can convert the CaSO4 in the fluorine-containing sludge into CaCO3, so as to facilitate the subsequent extraction of the Ca element therein.

[0100] There is no excessive limitation on the carbonate solution, and conventional carbonate solutions in the art, such as Na2CO3 solution, K2CO3 solution, etc., can be used.

[0101] Preferably, the carbonate solution is a Na2CO3 solution with a mass concentration of 10% to 30%.

[0102] Adding dispersant can make CaF2 particles evenly dispersed in the mixed system to prevent them from settling and agglomerating, which is not conducive to subsequent treatment. The dispersant can effectively dissolve organic impurities in fluorine-containing sludge. The coagulant, flocculant, etc. can be dissolved after mixing and coordination reaction of carbonate solution and dispersant, and then removed after solid-liquid separation.

[0103] The above-mentioned dispersant includes at least one of polyethylene glycol and polysorbate.

[0104] Furthermore, the polyethylene glycol includes at least one of polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 800.

[0105] Furthermore, the reaction temperature of step 1) is 40-60°C.

[0106] In another specific embodiment, the process further includes refining the fluorine-containing sludge before step 1) to facilitate the full reaction of the components in the fluorine-containing sludge.

[0107] The present invention does not limit the refinement treatment method, such as using a ball mill to refine the fluorine-containing sludge.

[0108] After being treated in step 1), the main components of the obtained impurity-free fluorine-containing sludge are CaF2, SiO2, CaCO3, Ca(OH)2, etc.

[0109] In step 2), the hydrofluoric acid solution acidification can convert CaCO3 and Ca(OH)2 in the fluorine-containing sludge into CaF2, and because the hydrofluoric acid solution promotes the dissolution of CaF2, it can make the dispersed fine CaF2 form a larger form of CaF2 in the hydrofluoric acid solution, reducing the severity of the HF reaction in the second acidification treatment; and the hydrofluoric acid reacts with SiO2 in the impurity-removed fluorine-containing sludge to produce SiF4 gas, thereby removing the solid SiO2 in the impurity-removed fluorine-containing sludge. The added hydrofluoric acid solution does not introduce other impurity ions during the reaction process.

[0110] Furthermore, the mass concentration of the hydrofluoric acid solution is 5% to 10%.

[0111] Furthermore, in step 2), the reaction temperature of the first acidification treatment is 20-35°C.

[0112] After the first acidification treatment, the mixed system is subjected to solid-liquid separation to obtain a solid product, namely crude calcium fluoride.

[0113] In step 3), crude calcium fluoride reacts with sulfuric acid to generate crude HF and calcium sulfate byproduct, wherein the sulfuric acid is a mixture of 98% sulfuric acid and 20% oleum.

[0114] There is A in the crude HF S Impurities, P impurities, S impurities, among which A S Elements, P elements and S elements exist in low-valent compound states.

[0115] In step 4), fluorine gas is used to convert the low-valent A S The element, P element and S element are oxidized to AsF5 high boiling product, PF5 and SF6 low boiling products respectively. AsF5 high boiling product can be separated from HF in this step, so the gas phase product is mainly HF and PF5 and SF6 low boiling product impurities.

[0116] Fluorine gas is used to oxidize impurities in the crude HF product without introducing other oxidant impurities.

[0117] Furthermore, the mass ratio of fluorine gas to crude HF is 0.01-0.03%.

[0118] Through the distillation treatment in step 5), the PF5 and SF6 low-boiling impurities can be separated from HF to obtain refined HF and a light gas phase, wherein the light gas phase contains SO2 and SiF4 in addition to a small amount of PF5 and SF6.

[0119] The method for treating fluorine-containing sludge of the present invention uses fluorine-containing sludge waste in the photovoltaic and photoelectric industries as raw materials, extracts and separates calcium fluoride and calcium salt in the fluorine-containing sludge through impurity removal treatment and a first acidification treatment, converts calcium fluoride into crude HF through a second acidification treatment, removes impurities from the crude HF through oxidation treatment and distillation treatment, obtains HF liquid with a high yield, and realizes resource utilization of fluorine-containing sludge.

[0120] In a specific implementation manner, before step 5), the method further comprises:

[0121] Performing a first condensation treatment on the gas phase product to obtain a condensate product;

[0122] returning part of the condensate product to participate in the oxidation treatment, and subjecting the remaining part of the condensate product to the refining treatment;

[0123] The volume ratio of the condensate product returned to participate in the oxidation treatment to the condensate product subjected to the refining treatment is 3-7.

[0124] By returning part of the condensate product to participate in the oxidation treatment, the unreacted low-valent A in the liquid product can be S Elements, P elements and S elements further react.

[0125] By setting a volume ratio of 3 to 7 between the condensate product returned for the oxidation treatment and the condensate product subjected to the refining treatment, the return of the condensate product can be promoted and the liquid flow rate in the reaction device can be increased.

[0126] In a specific embodiment, the second acidification treatment comprises:

[0127] pretreating the crude calcium fluoride and mixing it with sulfuric acid to obtain a solid-liquid mixture;

[0128] Performing acidification pretreatment on the solid-liquid mixture to obtain an acidified gas phase product and an acidified solid-liquid mixture;

[0129] The acidified solid-liquid mixture is subjected to acidification intermediate treatment and acidification post-treatment in sequence to obtain a first HF crude product;

[0130] The acidified gas phase product is fractionated to obtain a second HF crude product and an acidic heavy component;

[0131] Wherein, the HF crude product in step 4) includes a first HF crude product and a second HF crude product;

[0132] The temperature of the pretreatment is 150-200°C, the temperature of mixing with sulfuric acid is 50-60°C, the temperature of the acidification pre-treatment is 80-120°C, the temperature of the acidification treatment is 180-300°C, and the temperature of the acidification post-treatment is 150-200°C.

[0133] Before the crude calcium fluoride is mixed with sulfuric acid, the crude calcium fluoride is pretreated to remove moisture therein, thereby reducing the corrosion of the crude calcium fluoride to the reaction device during the reaction between the crude calcium fluoride and sulfuric acid. The crude calcium fluoride after the pretreatment is then mixed with sulfuric acid to obtain a solid-liquid mixture.

[0134] Furthermore, the pretreatment temperature is 150-200°C and the heating time is 2-4h.

[0135] The solid-liquid mixture is subjected to an acidification pretreatment, during which the crude calcium fluoride reacts with a small amount of sulfuric acid to obtain an acidified gas phase product and an acidified solid-liquid mixture.

[0136] Furthermore, during the acidification pretreatment process, the temperature of the acidification pretreatment is 80~120°C, the reaction time is 0.5~1h, the reaction temperature is gradient controlled, the initial temperature is 50~60°C, and the heating temperature is 80~120°C. The gradient control of the reaction temperature can slow down the reaction rate of the acidification pretreatment, promptly remove the gas generated by the reaction, and further prevent violent reactions during the acidification pretreatment process.

[0137] Afterwards, the acidified solid-liquid mixture is subjected to acidification intermediate treatment and acidification post-treatment in sequence to obtain a first HF crude product. The time for the acidification intermediate treatment and the acidification post-treatment is 1 to 2 hours.

[0138] The second acidification treatment adopts segmented heating, which can make full use of the heat of the reaction process and reduce energy consumption. The reaction progress is controlled by segmented heating, and the area with the strongest reaction corrosion is controlled in the acidification pre-treatment stage, avoiding corrosion of the equipment in the acidification mid-treatment and acidification post-treatment.

[0139] The acidified gas phase product is fractionated to obtain a second HF crude product and an acidic heavy component. The first HF crude product is mixed with the second HF crude product and enters a subsequent treatment process.

[0140] Setting different reaction temperatures during acidification treatment and after acidification treatment can control the reaction rate, make the reaction proceed smoothly and avoid violent reactions.

[0141] Furthermore, the temperature of the acidification treatment is 180-300° C., and the temperature of the acidification post-treatment is 150-200° C.; the reaction time of the acidification treatment and the acidification post-treatment is 1-2 h.

[0142] In a specific embodiment, after the acidic heavy component is purified, the purified product is used as the hydrofluoric acid solution to participate in the first acidification treatment.

[0143] The acidic heavy components are mainly HF and sulfuric acid solution. HF can be separated through purification treatment and can be configured into hydrofluoric acid solution for the first acidification treatment.

[0144] The above-mentioned purification treatment may specifically be distillation, or other commonly used purification treatment methods in the art.

[0145] In a specific embodiment, the light impurity gas phase in step 5) is subjected to a second condensation treatment to obtain a liquid phase product and gas phase impurities;

[0146] The liquid phase product is returned to participate in the distillation process; the volume ratio of the liquid phase product to the gas phase impurities is 2-5;

[0147] The gas phase impurities are absorbed by an absorbent to obtain by-products of calcium fluorosilicate and calcium sulfate.

[0148] In step 5), the light impurity gas phase contains HF, PF5, SF6, SO2, and SiF4. The light impurity gas phase is subjected to a second condensation treatment to obtain a liquid product containing HF, PF5, and SF6 and gas impurities containing SO2 and SiF4. The liquid product is returned to participate in the distillation treatment, and the HF contained in the liquid product is further separated. The gas impurities are absorbed by an absorbent to obtain by-products of calcium fluorosilicate and calcium sulfate. The gas impurity absorbent can specifically be water or lime water.

[0149] In a specific embodiment, the temperature of the impurity removal treatment in step 1) is 40-60°C;

[0150] Step) 2 The temperature of the first acidification treatment is 20-35°C;

[0151] Step) 3: The volume ratio of 98% sulfuric acid to 20% oleum is 1.5-2;

[0152] Step) 3: The mass ratio of the crude calcium fluoride to the acidic solvent is 1 to 1.4;

[0153] Step 4) The temperature of the oxidation treatment is 20-35°C;

[0154] The temperature of the first condensation treatment is 15~25℃;

[0155] The temperature of the second condensation treatment is 10-15°C.

[0156] By controlling the reaction temperature and material ratio of each step, the raw material cost and reaction efficiency can be taken into account.

[0157] A second aspect of the present invention provides a system for executing the above method, such as Figure 1 The method comprises an alkalization reactor 1, a first acidification reactor 2, a second acidification reactor 3, an oxidation tower 4 and a distillation tower 5;

[0158] The outlet of the alkalization reactor 1 is connected to the inlet of the first acidification reactor 2, the outlet of the first acidification reactor 2 is connected to the inlet of the second acidification reactor 3, the gas phase outlet of the second acidification reactor 3 is connected to the gas inlet of the oxidation tower 4, and the gas phase outlet of the oxidation tower 4 is connected to the inlet of the distillation tower 5.

[0159] In the system for executing the method for treating fluorine-containing sludge of the present invention, each reactor is reasonably connected to achieve the treatment of fluorine-containing sludge.

[0160] In a specific embodiment, Figure 2 and Figure 4 , further comprising a first condenser 6, the oxidation tower 4 and the distillation tower 5 are connected via the first condenser 6;

[0161] The gas phase outlet 407 of the oxidation tower 4 is located above the oxidation tower 4 , the gas phase outlet of the first condenser 6 is connected to the inlet of the distillation tower 5 , and the liquid phase outlet of the first condenser 6 is connected to the upper inlet of the oxidation tower 4 .

[0162] The liquid flowing out through the liquid phase outlet of the first condenser 6 enters from the upper liquid inlet 408 of the oxidation tower 4, and contacts in reverse with the fluorine gas entering from the lower fluorine gas inlet 406 of the oxidation tower 4. The fluorine gas is generated by the fluorine gas generator 10, achieving full contact between the gas and liquid materials, thereby making the reaction more complete.

[0163] Furthermore, the distillation tower 5 is made of stainless steel lined with fluoroplastics, which can prevent HF from corroding the metal material of the tower during the distillation process and causing HF pollution.

[0164] like Figure 4 In a specific embodiment, a reboiling plate 402 is provided at the bottom of the oxidation tower 4 , and the reboiling plate 402 is located below the gas inlet of the oxidation tower 4 .

[0165] The liquid condensed inside the oxidation tower 4 drips onto the reboiling pan 402, and the liquid is heated and vaporized again and then rises, mixed with the HF gas and rises to contact the mixed fluorine gas again in reverse, further promoting the utilization of the fluorine gas. In addition, the reboiling pan 402 heats the liquid dripping onto it, forming a complementary heating circulation condensate with the liquid in the circulation tank 405, and while vaporizing the condensate, it effectively prevents the high-boiling substances in the liquid tank from being carried into the mixed gas of the oxidation tower 4 again due to the excessively high temperature.

[0166] Furthermore, the reboiler tray 402 is densely covered with pores.

[0167] Furthermore, the temperature of the reboiler 402 is 30-40°C.

[0168] In another specific embodiment, a liquid distributor 403 is provided above the oxidation tower 4, and the liquid distributor 403 is located below the upper inlet.

[0169] The liquid distributor 403 sprays the liquid flowing out of the liquid phase outlet of the first condenser 6, and the liquid contacts the fluorine gas in reverse direction in the form of mist, further expanding the contact area between the gas and liquid materials.

[0170] Furthermore, a gas inlet and a gas distributor 404 are provided at a distance of 1 / 4 from the bottom, a liquid inlet and a liquid distributor 403 are provided at the top, and a packing layer 409 is provided between the gas distributor 404 and the liquid distributor 403 .

[0171] Furthermore, the filler layer 409 is a polytetrafluoroplastic particle layer.

[0172] In a specific embodiment, the oxidation tower 4 is further provided with a reboiler 410 for heating the crude HF product entering the oxidation tower 4 .

[0173] The gas distributor 404 and liquid distributor 403 provided in the oxidation tower can fully disperse the gas and liquid materials, so that the reaction materials can fully contact each other. The packing layer 409 can slow down the rising speed of the fluorine gas in the reaction tower, and also has the plate effect of rectification, increasing the contact surface with the HF gas and the condensation circulating liquid and the material rising resistance. The high-boiling and low-boiling substances after oxidation can be effectively separated from HF in the packing layer 409 and the reflux and condensation liquid circulation.

[0174] Furthermore, a circulation tank 405 is provided at the bottom for enriching and separating the heavy components generated during the oxidation treatment.

[0175] Furthermore, the heating temperature of the circulation tank is 20-30°C.

[0176] like Figure 3 In a specific embodiment, the second acidification reactor comprises a pre-reactor 301 and a rotary reactor 307 which are interconnected, the pre-reactor 301 and the rotary reactor 307 are detachably connected, the outlet of the first acidification reactor 2 is connected to the inlet of the pre-reactor 301, and the gas phase outlet of the rotary reactor 307 is connected to the inlet;

[0177] A scraper 304 is disposed on the rotating shaft of the pre-reactor 301, and the scraper 304 and the pre-reactor 301 rotate in opposite directions;

[0178] A slag return cylinder 309 is arranged on the rotating shaft of the rotary reactor 307, and the rotation direction of the slag return cylinder 309 and the rotary reactor 307 are opposite, and a material lifting piece 310 and a material blocking piece 311 bent in the opposite direction to the inlet of the pre-reactor 301 are arranged on the inner wall of the rotary reactor 307;

[0179] The rotary reaction furnace 307 is provided with electric heating devices at the furnace head and furnace tail, so as to realize the setting of different reaction temperatures for acidification treatment and acidification post-treatment. The reaction temperature distribution of the rotary reaction furnace 307 reasonably distributes the reaction area of ​​the rotary reaction furnace 307, greatly reduces the corrosion of the rotary reaction furnace 307, and increases the service life of the rotary reaction furnace 307.

[0180] The material output from the first acidification reactor 2 enters through the feed port 302 of the pre-reactor 301; sulfuric acid enters through the acid inlet 303; the gas generated by the acidification pre-treatment reaction is discharged through the gas phase outlet 305 of the pre-reactor 301; the gas generated by the acidification mid-treatment and acidification post-treatment reactions is discharged through the gas phase outlet 308 of the rotary reactor 307.

[0181] Furthermore, a negative pressure blower is provided in the pre-reactor 301 to discharge the gas generated by the reaction in time and prevent the gas generated by the violent reaction and the accompanying materials from clogging the pipeline.

[0182] Furthermore, the pre-reactor 301 and the rotary reactor 307 can be detachably connected, such as by threaded connection or snap connection. Figure 3 The pre-reactor 301 is connected to the rotary reactor 307 via a spiral connection port 306 .

[0183] During the second acidification treatment, the reaction is most intense in the pre-reactor 301 , and the corrosion to the pre-reactor 301 is also the greatest. By adopting a detachable connection method, the corroded pre-reactor 301 can be easily replaced, thereby preventing the entire system from stopping due to damage to the pre-reactor 301 .

[0184] In another specific embodiment, the material of the pre-reactor 301 is Hastelloy or Monel alloy, which can improve the corrosion resistance of the equipment; the material of the rotary reactor 307 is carbon steel or stainless steel.

[0185] After the fluorine-containing sludge is subjected to the impurity removal treatment and the first acidification treatment, the purified CaF2 particles obtained are fine and easy to form a sticky substance with sulfuric acid and adhere to the inner wall of the pre-reactor 301. A scraper 304 is arranged on the rotating shaft of the pre-reactor 301, and the scraper 304 and the pre-reactor 301 rotate in opposite directions, so that the material adhered to the inner wall can be continuously scraped off by the scraper 304 to prevent the material from accumulating in the pre-reactor 301.

[0186] A slag return cylinder 309 is arranged on the rotating shaft of the rotary reactor 307, and the rotation direction of the slag return cylinder 309 and the rotary reactor 307 are opposite, and a material lifting piece 310 and a material blocking piece 311 bent in the opposite direction to the entrance of the pre-reactor 301 are arranged on the inner wall of the rotary reactor 307, which play a role in stirring the materials in the rotary reactor 307. At the same time, the by-product CaSO4 of the second acidification treatment can be returned to the front of the rotary reactor 307 under the action of the slag return cylinder 309 and the material blocking piece 311, which can provide heat for the mixture of crude calcium fluoride and sulfuric acid at the end of the rotary reactor 307 on the one hand, and the dry CaSO4 slag can dilute the sticky mixture of crude calcium fluoride and sulfuric acid on the other hand, and prevent the mixture from forming a wall in the furnace.

[0187] A material lifting member 310 is provided in the rotary reactor 307. Under the action of the rotary reactor 307 rotating, the contact surface with the material in the rotary reactor 307 is expanded and a secondary paddle stirring effect is formed. The residual material that has not been completely reacted is stirred for a second time under the action of the material lifting member 310 and the material blocking member 311 to complete the reaction, and the HF gas contained therein can be released and separated at the same time.

[0188] Furthermore, the material lifting members 310 are arranged from the middle of the furnace body to the furnace tail and are evenly distributed. Furthermore, the surface of the material lifting members 310 is convex toward the furnace head, which can further expand the contact area with the material.

[0189] The internal design of the second acidification reactor 3 can increase the retention time of the material in the second acidification reactor, enhance the internal stirring effect, and reasonably utilize the generated CaSO4 to provide heat for the reaction, saving heat consumption, and diluting the reaction raw materials to prevent the material from agglomerating and sticking to the wall. Finally, the calcium sulfate formed in the second acidification reactor 3 is discharged through the slag outlet 312.

[0190] In a specific embodiment, a fractionation tower 7 is further included, and the gas phase outlet of the pre-reactor 301 is connected to the inlet of the fractionation tower 7, and the gas phase outlet of the fractionation tower 7 is connected to the inlet.

[0191] The fractionation tower 7 is used to fractionate the gas phase product obtained by the acidification pretreatment. The temperature of the tower body of the fractionation tower 7 is 35-40°C, and the temperature of the tower top is 25-35°C.

[0192] In a specific embodiment, a distiller 8 is further included, the liquid phase outlet of the fractionation tower 7 is communicated with the inlet of the distiller 8 , and the gas phase outlet of the distiller 8 is communicated with the inlet of the first acidification reactor 2 .

[0193] After the gas phase product is fractionated, a second HF crude product and an acidic heavy component are obtained. The acidic heavy component is treated by a distiller 8 to recover the HF therein. The recovered HF can be configured into a solution to supplement the hydrofluoric acid solution in the first acidification treatment.

[0194] In a specific embodiment, it also includes a second condenser 9, the distillation product outlet of the distillation tower 5 is connected to the inlet of the second condenser 9, the liquid product outlet of the second condenser 9 is connected to the inlet of the distillation tower 5, and the gas product outlet of the second condenser 9 is connected to the gas impurity treatment device.

[0195] The second condenser 9 is used to condense the distillation product. After condensation, HF, PF5 and SF6 in the distillation product are returned to the distillation tower 5 to separate HF, non-condensable gases SO2 and SiF4, and input them into the gas phase impurity treatment device to obtain by-products calcium fluorosilicate and calcium sulfate.

[0196] The present invention does not impose too many restrictions on the gas phase impurity treatment device, and conventional devices in the field can be used, such as a gas absorption device filled with water, a gas absorption device filled with lime water, etc.

[0197] In a specific embodiment, Figure 5 A liquid storage tank 501 is provided at the bottom of the distillation tower 5, and the liquid storage tank 501 is provided with a heating device.

[0198] Refined HF is formed in the liquid storage tank 501, and the liquid storage tank 501 is provided with a heating device to make the HF liquid obtained by boiling maintain a positive pressure in the distillation tower 5, and the evaporated HF in the tower can further form a circulation reflux with the materials in the tower.

[0199] Furthermore, the temperature of the liquid storage tank 501 is 18-30°C; the temperature of the top of the distillation tower is 15-20°C.

[0200] Furthermore, the distillation tower 5 is made of stainless steel lined with fluoroplastics, which can prevent HF from corroding the metal material of the distillation tower 5 during the distillation process and causing HF pollution.

[0201] The solution provided by the present invention is further described below in conjunction with specific embodiments.

[0202] Example 1

[0203] The specific steps of the treatment method of fluorine-containing sludge in this embodiment are as follows:

[0204] 1) 500 kg of fluorine-containing sludge is finely dispersed in a ball mill and then transported to an alkalization reactor. Polyethylene glycol 600 is mixed with 25% sodium carbonate solution to a concentration of 1% polyethylene glycol 600, added to the alkalization reactor, heated to 45°C and mixed and stirred, and the reaction time is controlled to 1.5 hours. After the pH value of the material reaches about neutral, the stirring rate is reduced to 1 / 50 of the original stirring rate and maintained for 3 hours; the impure fluorine-containing sludge is separated by solid-liquid separation, and it does not need to be washed or dried, and is transported to the first acidification reactor.

[0205] 2) Mix the impure fluorine-containing sludge with 5% hydrofluoric acid solution in the first acidification reactor, set the temperature of the acidification reactor to 30°C, and set the stirring speed to 500r / min, so that the reactants are suspended and fully stirred, and the acidification reaction is carried out for 1.5h. After solid-liquid separation, crude calcium fluoride and acidic filtrate are obtained, and the crude calcium fluoride can be used as a substitute for fluorite.

[0206] 3) The crude calcium fluoride is input into the pre-reactor of the second acidification reactor, heated to 200°C and maintained for 3 hours, cooled to the initial pre-reaction temperature of 55°C, and a mixed acid of 98% sulfuric acid and 20% oleum in a volume ratio of 1.5:1 is introduced, and the mass ratio of the mixed acid to the crude calcium fluoride is 1.1:1. After rotating reaction for 0.5 hours, the temperature is slowly raised to the pre-reaction temperature of 90°C and maintained for 0.5 hours to obtain a gas phase product and a solid-liquid mixed product.

[0207] The solid-liquid mixed product is transported to the rotary reactor for acidification treatment and post-acidification treatment to obtain the first HF crude product; the gas phase product is fractionated in a fractionation tower to obtain the second HF crude product and the acidic heavy component, the first HF crude product and the second HF crude product are mixed and transported to the oxidation tower, and the acidic heavy component is used to prepare the HF solution for the first acidification reaction after distillation treatment. Calcium sulfate solid is obtained at the tail of the rotary reactor.

[0208] The temperature of the distillation tower body is set at 35°C, and the temperature of the tower top is controlled at 30°C. The residence time of the solid-liquid mixed product in the rotary reactor is 1h. During the acidification treatment, the front end of the rotary reactor is controlled at 200°C, and after the acidification, the rear end of the rotary reactor is set at 160°C.

[0209] 4) The first HF crude product and the second HF crude product are heated at 30°C in a reboiler and then fed into a gas distributor of an oxidation tower, with a ventilation rate controlled at 20 kg / h; fluorine gas is fed into the oxidation tower at a rate of 5 g / h, the tower body temperature of the fluorination reaction is 30°C, the condensation temperature of the first condenser is 19°C, and the volume ratio of the liquid-phase oxidation product returned to the oxidation treatment to the liquid-phase oxidation product subjected to the refining treatment is 4.

[0210] 5) The material flowing out of the first condenser enters the distillation tower, and the distillation product is condensed by the second condenser. The obtained liquid is returned to the distillation tower, and the non-condensable gas is absorbed by water and lime water to obtain by-products such as calcium fluorosilicate and calcium sulfate.

[0211] The heating temperature of the liquid storage tank of the distillation tower is 25°C, the tower top temperature is 18°C, and the reflux ratio is controlled to be 3. After cyclic distillation, HF liquid is formed in the liquid storage tank to obtain 115Kg of HF liquid.

[0212] The preparation method of the present application can efficiently convert calcium fluoride in fluorine-containing sludge and realize resource processing of fluorine-containing sludge.

[0213] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for treating fluorine-containing sludge, characterized in that: The steps include: 1) mixing the fluorine-containing sludge, carbonate solution and dispersant to carry out impurity removal treatment, and obtaining impurity-removed fluorine-containing sludge when the pH value is 7-7.5; 2) subjecting the impurity-removed fluorine-containing sludge to a first acidification treatment with a hydrofluoric acid solution to obtain a crude calcium fluoride product; 3) subjecting the crude calcium fluoride to a second acidification treatment with sulfuric acid to obtain a crude HF product and calcium sulfate; the sulfuric acid comprises 98% sulfuric acid and 20% oleum; 4) oxidizing the crude HF product with fluorine gas to obtain a gas phase product; 5) performing rectification treatment on the gas phase product to obtain refined HF and light impurity gas phase; The second acidification treatment comprises: pretreating the crude calcium fluoride and mixing it with sulfuric acid to obtain a solid-liquid mixture; Performing acidification pretreatment on the solid-liquid mixture to obtain an acidified gas phase product and an acidified solid-liquid mixture; The acidified solid-liquid mixture is subjected to acidification intermediate treatment and acidification post-treatment in sequence to obtain a first HF crude product; The acidified gas phase product is fractionated to obtain a second HF crude product and an acidic heavy component; Wherein, the HF crude product in step 4) includes a first HF crude product and a second HF crude product; The temperature of the pretreatment is 150-200°C, the temperature of mixing with sulfuric acid is 50-60°C, the temperature of the acidification pre-treatment is 80-120°C, the temperature of the acidification treatment is 180-300°C, and the temperature of the acidification post-treatment is 150-200°C.

2. The method according to claim 1, characterized in that Before step 5), it also includes: Performing a first condensation treatment on the gas phase product to obtain a condensate product; returning part of the condensate product to participate in the oxidation treatment, and subjecting the remaining part of the condensate product to a refining treatment; The volume ratio of the condensate product returned to participate in the oxidation treatment to the condensate product subjected to the refining treatment is 3-7.

3. The method according to claim 1, characterized in that After purifying the acidic heavy component, the purified product is used as the hydrofluoric acid solution to participate in the first acidification treatment; and / or; performing a second condensation treatment on the light impurity gas phase in step 5) to obtain a liquid phase product and gas phase impurities; The liquid phase product is returned to participate in the distillation process; the volume ratio of the liquid phase product to the gas phase impurities is 2-5; The gas phase impurities are absorbed by an absorbent to obtain by-products of calcium fluorosilicate and calcium sulfate.

4. The method according to claim 3, characterized in that Step 1) The temperature of the impurity removal treatment is 40-60°C; And / or, the carbonate solution in step 1) includes at least one of a Na2CO3 solution and a K2CO3 solution; and / or, in step 1), the dispersant comprises at least one of polyethylene glycol and polysorbate; and / or, step) 2: the temperature of the first acidification treatment is 20-35°C; And / or, the volume ratio of 98% sulfuric acid to 20% oleum in step) 3 is 1.5-2; And / or, the mass ratio of the crude calcium fluoride product to the acidic solvent in step) 3 is 1 to 1.4; And / or, the temperature of the oxidation treatment in step) 4 is 20-35°C; And / or, the temperature of the first condensation treatment is 15-25°C; And / or, the temperature of the second condensation treatment is 10-15°C.

5. The method according to any one of claims 1 to 4, characterized in that: A system for performing the method includes an alkalization reactor, a first acidification reactor, a second acidification reactor, an oxidation column, and a distillation column; The outlet of the alkalization reactor is connected to the inlet of the first acidification reactor, the outlet of the first acidification reactor is connected to the inlet of the second acidification reactor, the gas phase outlet of the second acidification reactor is connected to the gas inlet of the oxidation tower, and the gas phase outlet of the oxidation tower is connected to the inlet of the distillation tower.

6. The method according to claim 5, characterized in that The system for performing the method further comprises a first condenser, the oxidation tower and the distillation tower being connected via the first condenser; The gas phase outlet of the oxidation tower is located above the oxidation tower, the gas phase outlet of the first condenser is connected to the inlet of the distillation tower, and the liquid phase outlet of the first condenser is connected to the upper inlet of the oxidation tower.

7. The method according to claim 6, characterized in that The second acidification reactor comprises a pre-reactor and a rotary reactor which are interconnected, the pre-reactor and the rotary reactor are detachably connected, the outlet of the first acidification reactor is connected to the inlet of the pre-reactor, and the gas phase outlet of the rotary reactor is connected to the inlet of the oxidation tower; A scraper is provided on the rotating shaft of the pre-reactor, and the rotation directions of the scraper and the pre-reactor are opposite; A slag return cylinder is arranged on the rotating shaft of the rotary reactor, and the rotation direction of the slag return cylinder and the rotary reactor are opposite, and a material lifting member and a material blocking member bent in the opposite direction to the inlet of the pre-reactor are arranged on the inner wall of the rotary reactor; The rotary reaction furnace is provided with electric heating devices at the furnace head and furnace tail respectively; And / or, it also includes a distillation tower, the gas phase outlet of the pre-reactor is connected to the inlet of the distillation tower, and the gas phase outlet of the distillation tower is connected to the inlet of the oxidation tower.

8. The method according to claim 7, characterized in that The system for performing the method further comprises a distiller, wherein the liquid phase outlet of the fractionation tower is connected to the inlet of the distiller, and the gas phase outlet of the distiller is connected to the inlet of the first acidification reactor.

9. The method according to any one of claims 6 to 8, characterized in that: The system for performing the method further includes a second condenser, the distillation product outlet of the distillation tower is connected to the inlet of the second condenser, the liquid product outlet of the second condenser is connected to the inlet of the distillation tower, and the gas product outlet of the second condenser is connected to the gas impurity processing device; And / or, a reboiling plate is arranged at the bottom of the oxidation tower, the reboiling plate is located below the gas inlet of the oxidation tower, and the temperature of the reboiling plate is 30-40° C.; And / or, the oxidation tower is provided with a gas inlet and a gas distributor at the bottom, the oxidation tower is provided with a liquid inlet, a liquid distributor and a circulation tank at the top, a packing layer is provided between the gas distributor and the liquid distributor, and the heating temperature of the circulation tank is 20-30° C.; And / or, a liquid storage tank is provided at the bottom of the distillation tower, and the temperature of the liquid storage tank is 18-30°C.

Citation Information

Patent Citations

  • Method for preparing electronic grade hydrofluoric acid

    CN102320573A

  • Method for treating fluorine-containing wastewater and recycling fluorine-containing sludge produced by treatment of fluorine-containing wastewater

    CN103848522A

  • Hydrofluoric acid mixing system and method

    CN108671878A

  • Method for extracting pure calcium fluoride from calcium fluoride sludge

    CN109775743A

  • Carbonation-activated clinker binder from incineration residues

    CN110475756A