A high-adhesion anti-aging tile adhesive and preparation method thereof

By using a combination of Portland cement, compound powder and other modified materials, a high-adhesion anti-aging ceramic tile adhesive is prepared, which solves the problems of insufficient anti-aging and fire-resistant performance of existing ceramic tile adhesives and achieves high-viscosity knotty and durable tile adhesive products.

CN118598616BActive Publication Date: 2024-10-11JIANGSU SHUNLICHENG NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411080321.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-11
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The anti-aging and fire-resistant properties of existing ceramic tile adhesives are insufficient, making it difficult to meet the needs for high adhesion and durability.

Method used

Using Portland cement, compound powder (prepared by mixing quartz sand and modified bentonite), redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose and other raw materials, through mixing and modification Process to prepare high-adhesion anti-aging ceramic tile adhesive.

Benefits of technology

It achieves high bonding performance, excellent anti-aging performance and reliable fire resistance, improves the quality and quality of tile adhesive, and is suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of building material production, specifically to a high-adhesive anti-aging tile adhesive and a preparation method thereof; the high-adhesive anti-aging tile adhesive is composed of the following raw materials by weight: 30 to 40 parts of silicate cement, 3 to 6 parts of compound powder, 10 to 14 parts of redispersible latex powder, 2 to 4 parts of reinforcing agent, 4 to 7 parts of fiber filler and 6 to 10 parts of hydroxypropyl methylcellulose; the present invention is to put each silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose into a mixing device for mixing and stirring, and after the mixing is completed, the material is discharged, and then the high-adhesive anti-aging tile adhesive is successively inspected and metered and packaged to finally obtain a finished product. The prepared high-adhesive anti-aging tile adhesive not only has good high-adhesive performance, but also has excellent anti-aging performance and reliable fire resistance, which effectively guarantees its quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material production, in particular to a high-adhesiveness anti-aging tile adhesive and a preparation method thereof. Background Art

[0002] In the construction process of tile laying, the traditional method is to bond tiles and walls mainly with cement. However, tiles laid directly with cement are prone to hollowing and falling off, and the maintenance cost is high. Tile adhesive is a new modern decoration material used to stick tiles, tiles, floor tiles and other decorative materials. With the continuous growth of people's needs, various tile adhesives have emerged, and the requirements for tile adhesives are getting higher and higher.

[0003] In the patent document with application number "CN202310296013.7" and titled "A high-adhesion anti-aging tile adhesive and its preparation method", it is recorded that "the high-adhesion anti-aging tile adhesive includes the following components in parts by weight: 80-120 parts of silicate cement, 80-120 parts of quartz sand, 20-40 parts of diatomaceous earth, 10-20 parts of redispersible latex powder, 2-10 parts of organic silicon-higher fatty acid composite water repellent, 1-5 parts of cellulose ether, and 1-2 parts of polycarboxylic acid water reducer. The preparation method The method comprises the following steps: mixing silicate cement, quartz sand and diatomaceous earth evenly, and then sequentially adding redispersible latex powder, organosilicon-higher fatty acid composite water repellent, cellulose ether and polycarboxylic acid water reducer and mixing evenly to obtain high-bonding anti-aging tile adhesive dry powder mortar. The present invention adopts a special organosilicon-higher fatty acid composite water repellent to significantly improve the bonding strength, waterproof performance and anti-aging performance of tile adhesive. This patent mainly relies on organosilicon-higher fatty acid composite water repellent to change the bonding strength and anti-aging performance of tile adhesive.

[0004] For example, the patent document with application number "CN2020112 9469.9" and titled "A high-adhesion cementitious material and high-strength permeable cement concrete material" states that "the high-adhesion cementitious material includes the following components and their weight contents: 100 parts of cement, 5-8 parts of microsilica powder, 28-32 parts of water, 0.9-1.1 parts of basalt fiber and 3.3-3 parts of reinforcing agent. .6 parts; the cement concrete material includes the following components and their weight contents: 4-5 parts of aggregate and 1 part of high-adhesion cementitious material. Compared with the prior art, the present invention is based on a composite method of physical filling-chemical modification. On the premise of ensuring that the modified permeable cement concrete does not produce cement mortar segregation, the amount of cement is increased; at the same time, the secondary filling effect of cement particles that do not participate in the hydration reaction and silica fume particles that do not participate in the secondary hydration reaction is utilized to eliminate macropores and homogenize the capillary pore distribution inside the cement mortar and at the cement-aggregate interface, significantly improving the mechanical properties of permeable concrete; at the same time, basalt fiber is used to further improve its mechanical and permeability properties. "This patent mainly relies on microsilica powder, basalt fiber and reinforcing agents to improve the performance of tile adhesive.

[0005] Although the tile adhesive manufactured by the above patent document has advantages such as excellent mechanical properties, its anti-aging and fire-resistant properties are relatively insufficient and still need to be further improved. Based on this, the present invention provides a high-adhesion anti-aging tile adhesive and a preparation method thereof to solve the above technical problems. Summary of the invention

[0006] The purpose of the present invention is to provide a high-adhesion anti-aging tile adhesive and a preparation method thereof. The prepared high-adhesion anti-aging tile adhesive not only has good high adhesion performance, but also has excellent anti-aging performance and reliable fire resistance, effectively ensuring its quality.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] The first aspect of the present invention provides a high-adhesion anti-aging tile adhesive, which is composed of the following raw materials in parts by weight: 30 to 40 parts of silicate cement, 3 to 6 parts of compound powder, 10 to 14 parts of redispersible latex powder, 2 to 4 parts of reinforcing agent, 4 to 7 parts of fiber filler and 6 to 10 parts of hydroxypropyl methylcellulose.

[0009] Furthermore, the composite powder is prepared by mixing quartz sand and modified bentonite in a mass ratio of 1:0.2-0.5.

[0010] Furthermore, the preparation process of the modified bentonite is as follows:

[0011] The bentonite is treated at 450-480°C for 80-100 minutes, and after cooling, a calcined product is obtained;

[0012] The calcined product is placed in 50% sulfuric acid at a dosage ratio of 0.22 to 0.32 g / mL for 10 to 12 hours, filtered, washed with deionized water 2 to 4 times, then dried at 70 to 90° C. for 15 to 25 hours, and crushed to 100 to 200 meshes to obtain bentonite powder;

[0013] The bentonite powder is placed in a modified solution at a dosage ratio of 0.02 to 0.08 g / mL, stirred at 120 to 160 r / min for 60 to 70 minutes, then ultrasonically treated for 20 to 30 minutes, and then treated in a water bath at 80 to 90° C. for 30 to 36 minutes. After filtration, it is dried at 70 to 90° C. to constant weight to obtain modified bentonite.

[0014] Furthermore, the modified solution is prepared by mixing 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 0.03 to 0.07:1.

[0015] Furthermore, the redispersible latex powder is selected from any one of ethylene-vinyl acetate copolymer powder and acrylate-styrene copolymer powder.

[0016] Furthermore, the preparation process of the enhancer is as follows:

[0017] The nano-β-eucryptite powder is ultrasonically dispersed in deionized water at a dosage ratio of 0.02 to 0.08 g / mL for 20 to 30 minutes, and after heating to 60 to 70° C., ammonium hexafluorosilicate and ammonia water are added thereto, and then stirred at 120 to 140 r / min for 40 to 46 minutes;

[0018] After the stirring is completed, the mixture is aged for 100 to 120 minutes, filtered, washed with deionized water for 2 to 4 times, and dried at a temperature of 70 to 90° C. to a constant weight to obtain a base material;

[0019] The obtained base material is sprayed with 3-aminopropyltriethoxysilane, and then treated at 40-50° C. for 50-60 minutes to obtain a reinforcing agent.

[0020] Furthermore, the amount of ammonium hexafluorosilicate added is 0.32-0.42% of the mass of the nano-β-eucryptite powder, and the amount of ammonia water added is 0.12-0.22% of the mass of the nano-β-eucryptite powder.

[0021] Furthermore, the spraying amount of the 3-aminopropyltriethoxysilane is 8-12% of the mass of the base material.

[0022] Furthermore, the fiber filler is compounded by basalt fiber and wollastonite fiber in a mass ratio of 1:0.5-0.8.

[0023] The second aspect of the present invention also provides a method for preparing a high-adhesion anti-aging tile adhesive, which is characterized by comprising the following steps:

[0024] Step 1: accurately weigh silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose, and put the silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose into a mixing device for mixing and stirring;

[0025] Wherein, the rotation speed of the mixing equipment is 220-240r / min, and the mixing time is 20-30min;

[0026] Step 2: After the mixing is completed, the materials are discharged, and then inspected, measured and packaged in sequence to finally obtain a high-adhesion anti-aging tile adhesive product.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] In the present invention, silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose are used as raw materials, wherein the compound powder is prepared by mixing quartz sand and modified bentonite, and each silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose are put into a mixing device for mixing and stirring, and after the mixing is completed, the material is discharged, and then the high-adhesion anti-aging tile adhesive is finally obtained through inspection and metering packaging processes. The high-adhesion anti-aging tile adhesive prepared by the present invention not only has good high-adhesion performance, but also has excellent anti-aging performance and reliable fire resistance, which effectively guarantees its quality. The high-adhesion anti-aging tile adhesive and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1: This example provides a high-adhesion anti-aging tile adhesive, which is composed of the following raw materials in parts by weight: 30 parts of silicate cement, 3 parts of compound powder, 10 parts of redispersible latex powder, 2 parts of reinforcing agent, 4 parts of fiber filler and 6 parts of hydroxypropyl methylcellulose.

[0031] In the examples, it should be noted that silicate cement was purchased from Shandong Jinhongshun Chemical Co., Ltd., and hydroxypropyl methylcellulose was purchased from Jinzhou Xingdong Building Materials Technology Co., Ltd.

[0032] The compound powder is prepared by mixing quartz sand and modified bentonite in a mass ratio of 1:0.2.

[0033] In this embodiment, it should be noted that the quartz sand was purchased from Lingshou County Haibin Mineral Products Trading Co., Ltd.

[0034] In addition, the preparation process of modified bentonite is as follows:

[0035] The bentonite was treated at 450°C for 80 minutes, and after cooling, a calcined product was obtained;

[0036] The calcined product was placed in 50% sulfuric acid at a dosage ratio of 0.22 g / mL for 10 h, filtered, washed twice with deionized water, dried at 70°C for 15 h, and crushed to 100 mesh to obtain bentonite powder;

[0037] Bentonite powder was placed in a modified solution at a dosage ratio of 0.02 g / mL, stirred at 120 r / min for 60 min, then ultrasonically treated for 20 min, and then treated in a water bath at 80° C. for 30 min. After filtration, it was dried at 70° C. to constant weight to obtain modified bentonite.

[0038] Furthermore, the modified solution is prepared by mixing 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 0.03:1.

[0039] In this embodiment, it should be noted that the bentonite was purchased from Jianping Cuican Bentonite Co., Ltd.

[0040] In addition, the redispersible latex powder is ethylene-vinyl acetate copolymer powder.

[0041] The preparation process of the enhancer is as follows:

[0042] The nano-β-eucryptite powder was ultrasonically dispersed in deionized water at a dosage of 0.02 g / mL for 20 min, and then the temperature was raised to 60°C, and ammonium hexafluorosilicate and ammonia water were added thereto, and then the mixture was stirred at 120 r / min for 40 min.

[0043] After stirring, the mixture was aged for 100 min, filtered, washed twice with deionized water, and dried at 70°C to constant weight to obtain a base material;

[0044] The obtained base material was sprayed with 3-aminopropyltriethoxysilane, and then treated at 40° C. for 50 minutes to obtain a reinforcing agent.

[0045] Furthermore, the amount of ammonium hexafluorosilicate added is 0.32% of the mass of the nano-β-eucryptite powder, and the amount of ammonia water added is 0.12% of the mass of the nano-β-eucryptite powder.

[0046] The spraying amount of 3-aminopropyltriethoxysilane is 8% of the base material mass.

[0047] The fiber filler is compounded by basalt fiber and wollastonite fiber in a mass ratio of 1:0.5.

[0048] In this embodiment, it should be noted that the basalt fiber was purchased from Jiangxi Shuobang New Material Technology Co., Ltd., and the wollastonite fiber was purchased from Jiangxi Huajietai Mineral Fiber Technology Co., Ltd.

[0049] In addition, this embodiment also provides a method for preparing a high-adhesion anti-aging tile adhesive, which is characterized by comprising the following steps:

[0050] Step 1: accurately weigh silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose, and put the silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose into a mixing device for mixing and stirring;

[0051] Among them, the speed of the mixing equipment is 220r / min, and the mixing time is 20min;

[0052] Step 2: After the mixing is completed, the materials are discharged, and then inspected, measured and packaged in sequence to finally obtain a high-adhesion anti-aging tile adhesive product.

[0053] Example 2: The preparation method of the high-adhesion anti-aging tile adhesive provided in this example is basically the same as that in Example 1, except that: the specific raw material composition and the specific preparation method of the high-adhesion anti-aging tile adhesive in this example are different; the specific raw material composition and the specific preparation method of the high-adhesion anti-aging tile adhesive in this example are as follows:

[0054] A high-adhesive anti-aging tile adhesive is composed of the following raw materials in parts by weight: 35 parts of silicate cement, 5 parts of compound powder, 12 parts of redispersible latex powder, 3 parts of reinforcing agent, 5 parts of fiber filler and 8 parts of hydroxypropyl methylcellulose.

[0055] In the examples, it should be noted that silicate cement was purchased from Shandong Jinhongshun Chemical Co., Ltd., and hydroxypropyl methylcellulose was purchased from Jinzhou Xingdong Building Materials Technology Co., Ltd.

[0056] The compound powder is prepared by mixing quartz sand and modified bentonite in a mass ratio of 1:0.3.

[0057] In this embodiment, it should be noted that the quartz sand was purchased from Lingshou County Haibin Mineral Products Trading Co., Ltd.

[0058] In addition, the preparation process of modified bentonite is as follows:

[0059] The bentonite was treated at 465°C for 90 minutes, and after cooling, a calcined product was obtained;

[0060] The calcined product was placed in 50% sulfuric acid at a dosage ratio of 0.27 g / mL for 11 h, filtered, washed with deionized water for 3 times, dried at 80°C for 20 h, and crushed to 150 mesh to obtain bentonite powder;

[0061] Bentonite powder was placed in a modified solution at a dosage ratio of 0.04 g / mL and stirred at 140 r / min for 65 min, then ultrasonically treated for 25 min, and then treated in a water bath at 85°C for 33 min. After filtration, it was dried at 80°C to constant weight to obtain modified bentonite.

[0062] Furthermore, the modified solution is prepared by mixing 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 0.04:1.

[0063] In this embodiment, it should be noted that the bentonite was purchased from Jianping Cuican Bentonite Co., Ltd.

[0064] In addition, the redispersible latex powder is made of acrylate-styrene copolymer powder.

[0065] The preparation process of the enhancer is as follows:

[0066] The nano-β-eucryptite powder was ultrasonically dispersed in deionized water at a dosage of 0.04 g / mL for 25 min, and then the temperature was raised to 65°C, and ammonium hexafluorosilicate and ammonia water were added thereto, and then the mixture was stirred at 130 r / min for 43 min.

[0067] After stirring, the mixture was aged for 110 min, filtered, washed with deionized water for 3 times, and dried at 80°C to constant weight to obtain a base material;

[0068] The obtained base material was sprayed with 3-aminopropyltriethoxysilane, and then treated at 45° C. for 55 minutes to obtain a reinforcing agent.

[0069] Furthermore, the amount of ammonium hexafluorosilicate added is 0.37% of the mass of the nano-β-eucryptite powder, and the amount of ammonia water added is 0.17% of the mass of the nano-β-eucryptite powder.

[0070] The spraying amount of 3-aminopropyltriethoxysilane is 10% of the base material mass.

[0071] The fiber filler is compounded by basalt fiber and wollastonite fiber in a mass ratio of 1:0.6.

[0072] In this embodiment, it should be noted that the basalt fiber was purchased from Jiangxi Shuobang New Material Technology Co., Ltd., and the wollastonite fiber was purchased from Jiangxi Huajietai Mineral Fiber Technology Co., Ltd.

[0073] In addition, this embodiment also provides a method for preparing a high-adhesion anti-aging tile adhesive, which is characterized by comprising the following steps:

[0074] Step 1: accurately weigh silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose, and put the silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose into a mixing device for mixing and stirring;

[0075] Among them, the speed of the mixing equipment is 230r / min, and the mixing time is 25min;

[0076] Step 2: After the mixing is completed, the materials are discharged, and then inspected, measured and packaged in sequence to finally obtain a high-adhesion anti-aging tile adhesive product.

[0077] Example 3: The preparation method of the high-adhesion anti-aging tile adhesive provided in this example is basically the same as that in Example 1, except that: the specific raw material composition and the specific preparation method of the high-adhesion anti-aging tile adhesive in this example are different; the specific raw material composition and the specific preparation method of the high-adhesion anti-aging tile adhesive in this example are as follows:

[0078] A high-adhesive anti-aging tile adhesive is composed of the following raw materials in parts by weight: 40 parts of silicate cement, 6 parts of compound powder, 14 parts of redispersible latex powder, 4 parts of reinforcing agent, 7 parts of fiber filler and 10 parts of hydroxypropyl methylcellulose.

[0079] In the examples, it should be noted that silicate cement was purchased from Shandong Jinhongshun Chemical Co., Ltd., and hydroxypropyl methylcellulose was purchased from Jinzhou Xingdong Building Materials Technology Co., Ltd.

[0080] The compound powder is prepared by mixing quartz sand and modified bentonite in a mass ratio of 1:0.5.

[0081] In this embodiment, it should be noted that the quartz sand was purchased from Lingshou County Haibin Mineral Products Trading Co., Ltd.

[0082] In addition, the preparation process of modified bentonite is as follows:

[0083] The bentonite was treated at 480°C for 100 minutes, and after cooling, a calcined product was obtained;

[0084] The calcined product was placed in 50% sulfuric acid at a dosage ratio of 0.32 g / mL for 12 h, filtered, washed with deionized water 4 times, dried at 90°C for 25 h, and crushed to 200 mesh to obtain bentonite powder;

[0085] Bentonite powder was placed in a modified solution at a dosage ratio of 0.08 g / mL and stirred at 160 r / min for 70 min, then ultrasonically treated for 30 min, and then treated in a 90° C. water bath for 36 min. After filtration, it was dried at 90° C. to constant weight to obtain modified bentonite.

[0086] Furthermore, the modified solution is prepared by mixing 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 0.07:1.

[0087] In this embodiment, it should be noted that the bentonite was purchased from Jianping Cuican Bentonite Co., Ltd.

[0088] In addition, the redispersible latex powder is ethylene-vinyl acetate copolymer powder.

[0089] The preparation process of the enhancer is as follows:

[0090] The nano-β-eucryptite powder was ultrasonically dispersed in deionized water at a dosage of 0.08 g / mL for 30 min, and then the temperature was raised to 70°C, and ammonium hexafluorosilicate and ammonia water were added thereto, and then the mixture was stirred at 140 r / min for 46 min.

[0091] After stirring, the mixture was aged for 120 min, filtered, washed with deionized water for 4 times, and dried at 90°C to constant weight to obtain a base material;

[0092] The obtained base material was sprayed with 3-aminopropyltriethoxysilane, and then treated at 50° C. for 60 minutes to obtain a reinforcing agent.

[0093] Furthermore, the amount of ammonium hexafluorosilicate added is 0.42% of the mass of the nano-β-eucryptite powder, and the amount of ammonia water added is 0.22% of the mass of the nano-β-eucryptite powder.

[0094] The spraying amount of 3-aminopropyltriethoxysilane is 12% of the base material mass.

[0095] The fiber filler is compounded by basalt fiber and wollastonite fiber in a mass ratio of 1:0.8.

[0096] In this embodiment, it should be noted that the basalt fiber was purchased from Jiangxi Shuobang New Material Technology Co., Ltd., and the wollastonite fiber was purchased from Jiangxi Huajietai Mineral Fiber Technology Co., Ltd.

[0097] In addition, this embodiment also provides a method for preparing a high-adhesion anti-aging tile adhesive, which is characterized by comprising the following steps:

[0098] Step 1: accurately weigh silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose, and put the silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose into a mixing device for mixing and stirring;

[0099] Among them, the speed of the mixing equipment is 240r / min, and the mixing time is 30min;

[0100] Step 2: After the mixing is completed, the materials are discharged, and then inspected, measured and packaged in sequence to finally obtain a high-adhesion anti-aging tile adhesive product.

[0101] Comparative Example 1: The difference from Example 1 is that in this example, an equal amount of bentonite is used instead of modified bentonite.

[0102] Comparative Example 2: The difference from Example 1 is that an equal amount of β-eucryptite powder is used to replace the reinforcing agent in this example.

[0103] Performance test: The high-adhesion anti-aging tile adhesive samples provided in Examples 1 to 3 and Comparative Examples 1 to 2 are marked as Examples 1 to 3 and Comparative Examples 1 to 2, respectively; and the relevant properties of the high-adhesion anti-aging tile adhesives provided in Examples 1 to 3 and Comparative Examples 1 to 2 are tested as follows:

[0104] 1. Tensile bond original strength test: The test method is JC / T547-2005, and the test steps are as follows: Add 25% (mass of tile adhesive) of water to the tile adhesive and mix it, then apply it evenly on the back of the C1 tile. After it becomes a transparent film, apply mortar on the surface of the backing glue, then stick it on the base surface and maintain it according to the standard test conditions of 7.1.

[0105] 2. Anti-aging test: The test method is JC / T547-2017, and the test steps are as follows: Add water to the tile adhesive, the amount of water added is 25% of the mass of the tile adhesive, stir evenly to obtain tile adhesive slurry. Let the tile adhesive slurry stand for 5 minutes, and then continue to stir for 15 seconds to obtain the sample to be tested.

[0106] 3. Fire resistance test: The test method is to mix each group of tile adhesive and water in a mass ratio of 5:1 and stir evenly until a paste without obvious particles is formed. Then, the paste is placed in a 100mm*100mm*100mm mold to form a standard test block. After 1 day, the mold is removed and the standard test block is allowed to stand in a natural environment for 28 days. Then, the standard test block is placed in an electric furnace at 1100℃ for 3 hours, cooled to room temperature with the furnace, taken out, and allowed to stand for 3 days. The conditions of each group of standard test blocks are recorded.

[0107] The obtained test data are recorded in Tables 1 to 3 below:

[0108]

[0109] By comparing and analyzing the relevant data in Tables 1 to 3, it can be seen that the high-adhesion anti-aging tile adhesive prepared by the present invention not only has good high-adhesion performance, but also has excellent anti-aging performance and reliable fire resistance, which effectively guarantees its quality. This shows that the high-adhesion anti-aging tile adhesive and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.

[0110] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0111] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high-adhesion anti-aging tile adhesive, characterized in that: The invention is composed of the following raw materials in parts by weight: 30 to 40 parts of silicate cement, 3 to 6 parts of compound powder, 10 to 14 parts of redispersible latex powder, 2 to 4 parts of reinforcing agent, 4 to 7 parts of fiber filler and 6 to 10 parts of hydroxypropyl methylcellulose; The composite powder is prepared by mixing quartz sand and modified bentonite in a mass ratio of 1:0.2-0.5; The preparation process of the modified bentonite is as follows: The bentonite is treated at 450-480°C for 80-100 minutes, and after cooling, a calcined product is obtained; The calcined product is placed in 50% sulfuric acid at a dosage ratio of 0.22 to 0.32 g / mL for 10 to 12 hours, filtered, washed with deionized water 2 to 4 times, then dried at 70 to 90° C. for 15 to 25 hours, and crushed to 100 to 200 meshes to obtain bentonite powder; The bentonite powder is placed in the modified solution at a dosage ratio of 0.02 to 0.08 g / mL, stirred at 120 to 160 r / min for 60 to 70 min, then ultrasonically treated for 20 to 30 min, and then treated in a water bath at 80 to 90° C. for 30 to 36 min, filtered, and dried at 70 to 90° C. to constant weight to obtain modified bentonite; The modified solution is prepared by mixing 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 0.03 to 0.07:1; The preparation process of the enhancer is as follows: The nano-β-eucryptite powder is ultrasonically dispersed in deionized water at a dosage ratio of 0.02 to 0.08 g / mL for 20 to 30 minutes, and after heating to 60 to 70° C., ammonium hexafluorosilicate and ammonia water are added thereto, and then stirred at 120 to 140 r / min for 40 to 46 minutes; After the stirring is completed, the mixture is aged for 100 to 120 minutes, filtered, washed with deionized water for 2 to 4 times, and dried at a temperature of 70 to 90° C. to a constant weight to obtain a base material; The obtained base material is sprayed with 3-aminopropyltriethoxysilane, and then treated at 40-50° C. for 50-60 minutes to obtain a reinforcing agent.

2. The high-adhesion anti-aging tile adhesive according to claim 1, characterized in that: The redispersible latex powder is selected from any one of ethylene-vinyl acetate copolymer powder and acrylate-styrene copolymer powder.

3. The high-adhesion anti-aging tile adhesive according to claim 1, characterized in that: The amount of ammonium hexafluorosilicate added is 0.32-0.42% of the mass of the nano-β-eucryptite powder, and the amount of ammonia water added is 0.12-0.22% of the mass of the nano-β-eucryptite powder.

4. The high-adhesion anti-aging tile adhesive according to claim 1, characterized in that: The spraying amount of the 3-aminopropyltriethoxysilane is 8-12% of the mass of the base material.

5. The high-adhesion anti-aging tile adhesive according to claim 1, characterized in that: The fiber filler is compounded by basalt fiber and wollastonite fiber in a mass ratio of 1:0.5-0.

8.

6. The method for preparing a high-adhesion anti-aging tile adhesive according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: accurately weigh silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose, and put the silicate cement, compound powder, redispersible latex powder, reinforcing agent, fiber filler and hydroxypropyl methylcellulose into a mixing device for mixing and stirring; Wherein, the rotation speed of the mixing equipment is 220-240r / min, and the mixing time is 20-30min; Step 2: After the mixing is completed, the materials are discharged, and then inspected, measured and packaged in sequence to finally obtain a high-adhesion anti-aging tile adhesive product.