A concrete thin layer repair material and its preparation process
Through the combination of modified composite fiber and nano-silver antibacterial powder and other components, the strength and durability of concrete thin-layer repair materials are improved, solving the problem of insufficient strength of concrete thin-layer repair materials in the existing technology, and achieving high-performance repair Effect.
Patent Information
- Application Number
- CN202411081474.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing concrete thin-layer repair materials are difficult to obtain high strength in a short period of time, and are easily damaged after being used for a period of time. They cannot effectively improve the durability of concrete and the service life of buildings.
A thin-layer concrete repair material is used, which includes sulphoaluminate cement, Portland cement, high-performance expansion agent, modified composite fiber and nano-silver antibacterial powder. Through the combination of modified composite fiber and carbon nanotubes, Combining to improve the overall strength and ductility of composite fibers, and through a reasonable combination of components, the compressive strength and bonding strength of concrete repair materials can be significantly improved.
It realizes that concrete repair materials can obtain higher strength in a shorter period of time, significantly improving the 2h compressive strength, 3d compressive strength and 3d positive tensile bonding strength, meeting the needs of high-performance concrete repair materials and extending the life of the building. service life.
Smart Images

Figure CN118598621B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete thin layer repair, and in particular to a concrete thin layer repair material and a preparation process thereof. Background Art
[0002] In the modern construction industry, cement concrete is the most widely used building material in construction projects. Generally speaking, concrete structures have good long-term performance and high durability. However, with the increase of service life and some other internal or external factors, the durability of cement concrete materials will decrease. For example, various physical, chemical and biological factors in nature will aggravate the damage of concrete. Even some newly built concrete projects will cause cracks, holes, honeycombs, pockmarks and other diseases, and even collapse if the design, construction and maintenance methods are unreasonable.
[0003] In the use scenarios of concrete, thin layers of concrete are most vulnerable to damage. Thin layers of concrete use less concrete and are often damaged faster than other concrete over a long period of time. In order to ensure the normal use of concrete, these thin layers of concrete need to be repaired, and repair materials are needed. Existing thin layer concrete repair materials tend to use ordinary Portland cement, water reducers and other admixtures for repair. It is difficult for thin layer repair materials to obtain high strength in a short period of time, and they cannot achieve high strength after molding. They are easily damaged after a period of use.
[0004] In order to improve the durability of concrete and extend the service life of buildings, it is of great significance to develop and apply a high-strength, high-pressure concrete thin layer repair material. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a concrete thin layer repair material and a preparation process thereof to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A concrete thin layer repair material comprises the following components by weight: component A: 280-320 parts of sulphoaluminate cement, 30-70 parts of silicate cement, 5-35 parts of high-performance expansion agent, 30-70 parts of admixture, 550-600 parts of fine aggregate, 0.2-0.6 parts of polycarboxylic acid water reducer and 0.5-2 parts of retarder; component B: 300-400 parts of water, 30-60 parts of modified composite fiber, 0.5-2 parts of inorganic dispersant, 0.2-1 parts of defoamer, 0.1-0.5 parts of wetting agent, 0.5-2 parts of antifreeze agent, 3-10 parts of nano silver antibacterial powder, 20-70 parts of water-based inorganic resin, 5-10 parts of lithium silicate, 5-10 parts of potassium silicate, 3-10 parts of redispersible latex powder and 0.2-1 parts of thickener.
[0008] Furthermore, the modified composite fiber is prepared by the following method:
[0009] S101, grinding polypropylene particles and polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder in a 2 mol / L hexadecyltrimethylammonium bromide solution and soaking them for 0.5-2 h, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder;
[0010] S102, blending the mixed powder obtained in step S101 with methyl cellulose and ammonium bicarbonate respectively and stirring them evenly, and melting the blended mixture in an extruder and stretching it to form a composite fiber;
[0011] S103, soaking the composite fiber obtained in step S102 in 25% ammonia water for 1-2 hours and then drying, dispersing the dried product in acetone, adding modified carbon nanotubes and blending for 2-4 hours, then adding bisphenol A type epoxy resin and heating and blending for 0.5-3 hours at a heating temperature of 40-80°C, filtering and drying to obtain the modified composite fiber.
[0012] Furthermore, in step S101, the mass ratio of the polypropylene powder to the polyethylene powder is 1:(1-3), and the mass ratio of the mixed powder to the hexadecyltrimethylammonium bromide solution is 1:(5-15).
[0013] Furthermore, in step S102, the mass ratio of ammonium bicarbonate, methyl cellulose and mixed powder is 1:(1-3):(10-20).
[0014] Furthermore, the mass ratio of the sum of the mass of the polypropylene particles and the polyethylene particles in step S101 to the mass of the modified carbon nanotubes, bisphenol A epoxy resin, acetone and ammonia water in step S103 is 1:(0.1-0.2):(0.4-0.5):(3-4):(8-12).
[0015] Furthermore, the modified carbon nanotubes in step S103 are prepared by the following steps:
[0016] S201, dispersing the carbon nanotubes into a mixed solution of sodium hydroxide and sodium dodecyl sulfate and soaking for 1-3 hours to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L;
[0017] S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and then calcining it in a muffle furnace at a temperature of 400-550°C for 2-5 hours to obtain modified carbon nanotubes.
[0018] Furthermore, in step S201, the mass ratio of the carbon nanotubes to the mixed solution of sodium hydroxide and sodium dodecyl sulfate is 1:8.
[0019] Furthermore, the water-based inorganic resin is selected as the water-based inorganic special resin with model number E777-4, the inorganic dispersant is selected as the silicate coating dispersant with model number DISPERSOGEN SPS, the thickener is selected as the polyurethane thickener with model number AMS-201, the redispersible latex powder is selected as the redispersible latex powder with model number ZN-800T, the defoamer is selected as the defoamer with model number DE-1226, and the wetting agent is selected as the wetting agent with model number KMT-7055.
[0020] Furthermore, the admixture is one of fly ash, slag powder, and silica ash, the fine aggregate is river sand with a particle size of 1-5 mm, the antifreeze is one of sodium nitrite, calcium chloride, and sodium chloride, the retarder is one of tartaric acid, potassium sodium tartrate, boric acid, borax, citric acid, and sodium gluconate, the high-performance expansion agent is one of calcium expansion agent, calcium-magnesium composite expansion agent, and calcium stearate, the modulus of the lithium silicate is 3.6-4.0, and the modulus of the potassium silicate is 2.5-3.0.
[0021] A preparation process for the above-mentioned concrete thin layer repair material comprises the following steps:
[0022] S1. Add sulphoaluminate cement, silicate cement, high-performance expansion agent, admixture, fine aggregate, polycarboxylate water reducer and retarder to mixer A in proportion, stir and mix evenly to obtain component A of concrete thin layer repair material;
[0023] S2, adding water, wetting agent, inorganic dispersant, defoamer, antifreeze agent and modified composite fiber to mixer B in proportion, with a stirring speed of 1300 r / min and a stirring time of 15 minutes;
[0024] S3, continue to add nano silver antibacterial powder into mixer B in proportion, stirring at a speed of 1300 r / min for 15 minutes;
[0025] S4, continue to add water-based inorganic resin, lithium silicate and potassium silicate into mixer B in proportion, stirring at a speed of 300 r / min for 15 minutes;
[0026] S5. Continue to add the redispersed latex powder into the mixer B in proportion, stirring at a speed of 300 r / min for 10 minutes;
[0027] S6. Continue to add thickener to mixer B in proportion, stirring at a speed of 300 r / min, and obtain component B of concrete thin layer repair material after stirring for 10 minutes;
[0028] S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The present invention further optimizes the composite fiber, and through the modification of the composite fiber and the carbon nanotubes, the carbon nanotubes and the composite fiber are efficiently combined with each other, thereby improving the overall strength of the composite fiber, improving the ductility and strength of the composite fiber, and enabling the composite fiber to better act in the repair material, ensuring that the repair material forms a sufficiently high strength after curing;
[0031] 2. Through the reasonable combination of various components in the present invention, the 2h compressive strength, 3d compressive strength and 3d tensile bonding strength of the concrete repair material are significantly improved. The repair material can obtain higher strength in a shorter time and can meet people's demand for high-performance concrete repair materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A process flow chart for preparing a concrete thin layer repair material according to the present invention;
[0033] Figure 2 The process flow chart of preparing the modified composite fiber of the present invention;
[0034] Figure 3 The present invention is a process flow chart for preparing modified carbon nanotubes. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] See also Figure 1-3 , the present invention provides a technical solution:
[0037] Example 1
[0038] A concrete thin layer repair material is prepared by the following steps:
[0039] S1. Add 29 kg of sulphoaluminate cement, 5.5 kg of silicate cement, 2.5 kg of calcium-magnesium composite expansion agent, 5 kg of slag powder, 57 kg of river sand with a particle size of 2 mm, 0.04 kg of polycarboxylate water reducer and 0.15 kg of potassium sodium tartrate into mixer A in sequence, stir and mix evenly to obtain component A of concrete thin layer repair material;
[0040] S2, add 35kg water, 0.04kg wetting agent, 0.1kg inorganic dispersant, 0.07kg defoamer, 0.1kg sodium chloride and 5kg modified composite fiber to the mixer B in sequence, with a stirring speed of 1300 r / min and a stirring time of 15 minutes;
[0041] S3, continue to add 1kg of nano silver antibacterial powder into mixer B, stirring at a speed of 1300 r / min, and stir for 15 minutes;
[0042] S4, to the mixer B, 6 kg of water-based inorganic resin, 0.8 kg of lithium silicate with a modulus of 3.8 and 0.8 kg of potassium silicate with a modulus of 3 were added, the stirring speed was 300 r / min, and the stirring time was 15 minutes;
[0043] S5, add 0.9 kg of redispersible latex powder to mixer B, stirring at a speed of 300 r / min for 10 minutes;
[0044] S6. Continue to add 0.08 kg of thickener to mixer B at a stirring speed of 300 r / min, and stir for 10 minutes to obtain component B of the concrete thin layer repair material;
[0045] S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material;
[0046] The modified composite fiber is prepared by the following steps:
[0047] S101, grinding 2 kg of polypropylene particles and 3 kg of polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder into 50 kg of 2 mol / L hexadecyltrimethylammonium bromide solution and soaking for 1.5 h, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder;
[0048] S102, blending the mixed powder obtained in step S101 with 1.5 kg of methyl cellulose and 0.8 kg of ammonium bicarbonate respectively and stirring them evenly, and melting the blended mixture in an extruder and stretching it to form a composite fiber;
[0049] S103, soaking the composite fiber obtained in step S102 in 52 kg of 25% ammonia water for 1.5 hours and then drying, dispersing the dried product in 18 kg of acetone, adding 0.75 kg of modified carbon nanotubes and blending for 4 hours, then adding 2.3 kg of bisphenol A epoxy resin and heating and blending for 2.5 hours at a heating temperature of 60° C., filtering and drying to obtain the modified composite fiber;
[0050] The modified carbon nanotubes are prepared by the following steps:
[0051] S201, dispersing 1 kg of carbon nanotubes into 8 kg of a mixed solution of sodium hydroxide and sodium dodecyl sulfate and soaking for 2 hours to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L;
[0052] S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and calcining it in a muffle furnace at a temperature of 450°C for 4 hours to obtain modified carbon nanotubes.
[0053] Example 2
[0054] A concrete thin layer repair material is prepared by the following steps:
[0055] S1. Add 32 kg of sulphoaluminate cement, 7 kg of silicate cement, 3.5 kg of calcium expansion agent, 7 kg of slag powder, 60 kg of river sand with a particle size of 1 mm, 0.06 kg of polycarboxylate water reducer and 0.2 kg of borax into mixer A in sequence, stir and mix evenly to obtain component A of concrete thin layer repair material;
[0056] S2, add 40kg water, 0.05kg wetting agent, 0.2kg inorganic dispersant, 0.1kg defoamer, 0.2kg calcium chloride and 6kg modified composite fiber to the mixer B in sequence, with a stirring speed of 1300 r / min and a stirring time of 15 minutes;
[0057] S3, continue to add 1kg of nano silver antibacterial powder into mixer B, stirring at a speed of 1300 r / min, and stir for 15 minutes;
[0058] S4, continue to add 7kg of water-based inorganic resin, 1kg of lithium silicate with a modulus of 3.6, and 1kg of potassium silicate with a modulus of 2.5 into mixer B, with a stirring speed of 300 r / min and a stirring time of 15 minutes;
[0059] S5, continue to add 1kg of redispersible latex powder into mixer B, stirring at a speed of 300 r / min, and stir for 10 minutes;
[0060] S6. Continue to add 0.1 kg of thickener to the mixer B at a stirring speed of 300 r / min, and stir for 10 minutes to obtain the concrete thin layer repair material component B;
[0061] S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material;
[0062] The modified composite fiber is prepared by the following steps:
[0063] S101, grinding 2 kg of polypropylene particles and 6 kg of polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder into 120 kg of 2 mol / L hexadecyltrimethylammonium bromide solution and soaking for 2 h, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder;
[0064] S102, blending the mixed powder obtained in step S101 with 2.4 kg of methyl cellulose and 0.8 kg of ammonium bicarbonate respectively and stirring them evenly, and melting the blended mixture in an extruder and stretching it to form a composite fiber;
[0065] S103, soaking the composite fiber obtained in step S102 in 96 kg of 25% ammonia water for 2 hours and then drying, dispersing the dried product in 32 kg of acetone, adding 1.6 kg of modified carbon nanotubes and blending for 4 hours, then adding 4 kg of bisphenol A epoxy resin and heating and blending for 3 hours at a heating temperature of 80° C., filtering and drying to obtain the modified composite fiber;
[0066] The modified carbon nanotubes are prepared by the following steps:
[0067] S201, dispersing 2 kg of carbon nanotubes into a mixed solution of 16 kg of sodium hydroxide and sodium dodecyl sulfate and soaking for 3 hours to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L;
[0068] S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and calcining it in a muffle furnace at a temperature of 550°C for 5 hours to obtain modified carbon nanotubes.
[0069] Example 3
[0070] A concrete thin layer repair material is prepared by the following steps:
[0071] S1. Add 30 kg of sulphoaluminate cement, 6 kg of silicate cement, 2.5 kg of calcium-magnesium composite expansion agent, 5 kg of fly ash, 58 kg of river sand with a particle size of 5 mm, 0.05 kg of polycarboxylate water reducer and 0.15 kg of potassium sodium tartrate into mixer A in sequence, stir and mix evenly to obtain component A of concrete thin layer repair material;
[0072] S2, 36kg water, 0.03kg wetting agent, 0.12kg inorganic dispersant, 0.08kg defoamer, 0.14kg sodium nitrite and 4.8kg modified composite fiber were added to the mixer B in sequence, with a stirring speed of 1300 r / min and a stirring time of 15 minutes;
[0073] S3, continue to add 0.8kg of nano silver antibacterial powder into mixer B, stirring at a speed of 1300 r / min, and stir for 15 minutes;
[0074] S4, add 5.5kg water-based inorganic resin, 0.7kg modulus 4 lithium silicate, 0.8kg modulus 3.2 potassium silicate into mixer B, stirring speed is 300 r / min, stirring time is 15 minutes;
[0075] S5, add 0.8 kg of redispersible latex powder to mixer B, stirring at a speed of 300 r / min for 10 minutes;
[0076] S6. Continue to add 0.09 kg of thickener to mixer B at a stirring speed of 300 r / min, and stir for 10 minutes to obtain component B of the concrete thin layer repair material;
[0077] S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material;
[0078] The modified composite fiber is prepared by the following steps:
[0079] S101, grinding 2 kg of polypropylene particles and 4 kg of polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder into 60 kg of 2 mol / L hexadecyltrimethylammonium bromide solution and soaking for 1.6 hours, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder;
[0080] S102, blending the mixed powder obtained in step S101 with 1.8 kg of methyl cellulose and 0.6 kg of ammonium bicarbonate respectively and stirring them evenly, and melting the blended mixture in an extruder and stretching it to form a composite fiber;
[0081] S103, soaking the composite fiber obtained in step S102 in 48 kg of 25% ammonia water for 1 hour and then drying, dispersing the dried product in 18 kg of acetone, adding 0.6 kg of modified carbon nanotubes and blending for 2 hours, then adding 2.4 kg of bisphenol A epoxy resin and heating and blending for 0.5 hours at a heating temperature of 40° C., filtering and drying to obtain the modified composite fiber;
[0082] The modified carbon nanotubes are prepared by the following steps:
[0083] S201, dispersing 1 kg of carbon nanotubes into 5 kg of a mixed solution of sodium hydroxide and sodium dodecyl sulfate and soaking for 2.5 hours to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L;
[0084] S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and then calcining it in a muffle furnace at a temperature of 400°C for 4 hours to obtain modified carbon nanotubes.
[0085] Example 4
[0086] A concrete thin layer repair material is prepared by the following steps:
[0087] S1. Add 28 kg of sulphoaluminate cement, 3 kg of silicate cement, 0.5 kg of calcium-magnesium composite expansion agent, 3 kg of silica powder, 55 kg of river sand with a particle size of 3 mm, 0.02 kg of polycarboxylate water reducer and 0.05 kg of citric acid into mixer A in sequence, stir and mix evenly to obtain component A of concrete thin layer repair material;
[0088] S2, add 30kg water, 0.01kg wetting agent, 0.05kg inorganic dispersant, 0.02kg defoamer, 0.05kg sodium chloride and 3kg modified composite fiber to the mixer B in sequence, with a stirring speed of 1300 r / min and a stirring time of 15 minutes;
[0089] S3, add 0.3kg of nano silver antibacterial powder to mixer B, stir at a speed of 1300 r / min, and stir for 15 minutes;
[0090] S4, add 2kg water-based inorganic resin, 0.5kg modulus 3.8 lithium silicate, 0.5kg modulus 3 potassium silicate to mixer B, stirring speed is 300 r / min, stirring time is 15 minutes;
[0091] S5, add 0.3kg of redispersible latex powder to mixer B, stir at a speed of 300 r / min, and stir for 10 minutes;
[0092] S6. Continue to add 0.02 kg of thickener to mixer B at a stirring speed of 300 r / min, and stir for 10 minutes to obtain component B of the concrete thin layer repair material;
[0093] S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material;
[0094] The modified composite fiber is prepared by the following steps:
[0095] S101, grinding 2 kg of polypropylene particles and 2 kg of polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder into 20 kg of 2 mol / L hexadecyltrimethylammonium bromide solution and soaking for 0.5 h, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder;
[0096] S102, blending the mixed powder obtained in step S101 with 0.2 kg of methyl cellulose and 0.2 kg of ammonium bicarbonate respectively and stirring them evenly, and melting the blended mixture in an extruder and stretching it to form a composite fiber;
[0097] S103, soaking the composite fiber obtained in step S102 in 35 kg of 25% ammonia water for 2 hours and then drying, dispersing the dried product in 14 kg of acetone, adding 0.5 kg of modified carbon nanotubes and blending for 3 hours, then adding 1.7 kg of bisphenol A epoxy resin and heating and blending for 2 hours at a heating temperature of 50° C., filtering and drying to obtain the modified composite fiber;
[0098] The modified carbon nanotubes are prepared by the following steps:
[0099] S201, dispersing 1 kg of carbon nanotubes into 8 kg of a mixed solution of sodium hydroxide and sodium dodecyl sulfate and soaking for 1 hour to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L;
[0100] S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and calcining it in a muffle furnace at a temperature of 450°C for 2 hours to obtain modified carbon nanotubes.
[0101] Example 5
[0102] A concrete thin layer repair material is prepared by the following steps:
[0103] S1. Add 30 kg of sulphoaluminate cement, 6 kg of silicate cement, 2.5 kg of calcium stearate, 5 kg of slag powder, 58 kg of river sand with a particle size of 2 mm, 0.06 kg of polycarboxylate water reducer and 0.2 kg of potassium sodium tartrate into mixer A in sequence, stir and mix evenly to obtain component A of concrete thin layer repair material;
[0104] S2, 38kg water, 0.03kg wetting agent, 0.2kg inorganic dispersant, 0.07kg defoamer, 0.2kg antifreeze and 6kg modified composite fiber were added to the mixer B in sequence, with a stirring speed of 1300 r / min and a stirring time of 15 minutes;
[0105] S3, add 0.6 kg of nano silver antibacterial powder to mixer B, stir at a speed of 1300 r / min, and stir for 15 minutes;
[0106] S4, to the mixer B, 5kg of water-based inorganic resin, 0.8kg of lithium silicate with a modulus of 3.8 and 0.8kg of potassium silicate with a modulus of 3 were added, the stirring speed was 300 r / min, and the stirring time was 15 minutes;
[0107] S5, continue to add 1kg of redispersible latex powder into mixer B, stirring at a speed of 300 r / min, and stir for 10 minutes;
[0108] S6. Continue to add 0.1 kg of thickener to the mixer B at a stirring speed of 300 r / min, and stir for 10 minutes to obtain the concrete thin layer repair material component B;
[0109] S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material;
[0110] The modified composite fiber is prepared by the following steps:
[0111] S101, grinding 2 kg of polypropylene particles and 5 kg of polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder into 65 kg of 2 mol / L hexadecyltrimethylammonium bromide solution and soaking for 1 hour, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder;
[0112] S102, blending the mixed powder obtained in step S101 with 0.7 kg of methyl cellulose and 0.4 kg of ammonium bicarbonate respectively and stirring them evenly, and melting the blended mixture in an extruder and stretching it to form a composite fiber;
[0113] S103, soaking the composite fiber obtained in step S102 in 60 kg of 25% ammonia water for 2 hours and then drying, dispersing the dried product in 25 kg of acetone, adding 1.1 kg of modified carbon nanotubes and blending for 2 hours, then adding 3.1 kg of bisphenol A epoxy resin and heating and blending for 3 hours at a heating temperature of 60° C., filtering and drying to obtain the modified composite fiber;
[0114] The modified carbon nanotubes are prepared by the following steps:
[0115] S201, dispersing 2 kg of carbon nanotubes into a mixed solution of 16 kg of sodium hydroxide and sodium dodecyl sulfate and soaking for 3 hours to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L;
[0116] S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and calcining it in a muffle furnace at a temperature of 500° C. for 5 hours to obtain modified carbon nanotubes
[0117] Comparative Example 1
[0118] The difference between Comparative Example 1 and Example 1 is that step S201 and step S202 are omitted, thereby canceling the modification process of carbon nanotubes, and ordinary carbon nanotubes are directly added in step S103.
[0119] Comparative Example 2
[0120] The difference between Comparative Example 2 and Example 1 is that step S101 is omitted, thereby eliminating the step of treating the polyethylene powder and the polypropylene powder with the hexadecyltrimethylammonium bromide solution, and the remaining steps are exactly the same as those in Example 1.
[0121] Comparative Example 3
[0122] The difference between Comparative Example 3 and Example 1 is that step S102 is omitted, thereby eliminating the addition of ammonium bicarbonate and methyl cellulose, and the remaining steps are exactly the same as those of Example 1.
[0123] Comparative Example 4
[0124] The difference between Comparative Example 4 and Example 1 is that step S103 is omitted, thereby eliminating the process of soaking the composite fiber in ammonia water, and the remaining steps are exactly the same as those in Example 1.
[0125] Comparative Example 5
[0126] The difference between Comparative Example 4 and Comparative Example 1 is that step S101 is omitted, thereby eliminating the step of treating the polyethylene powder and the polypropylene powder with the hexadecyltrimethylammonium bromide solution, and step S102 is omitted, thereby eliminating the addition of ammonium bicarbonate and methyl cellulose, and step S103 is further omitted, thereby eliminating the process of soaking the composite fiber in ammonia water, and the remaining steps are exactly the same as those in Comparative Example 1.
[0127] The aqueous inorganic resin used in the above-mentioned embodiments is a water-based inorganic special resin of model E777-4, the inorganic dispersant is a silicate coating dispersant of model DISPERSOGEN SPS, the thickener is a polyurethane thickener of model AMS-201, the redispersible latex powder is a redispersible latex powder of model ZN-800T, the defoamer is a defoamer of model DE-1226, and the wetting agent is a wetting agent of model KMT-7055.
[0128] 10 portions of concrete thin layer repair materials were prepared through the above-mentioned Examples 1-5 and Comparative Examples 1-5, respectively. At room temperature, when the initial setting time of the concrete thin layer repair materials was 30 minutes, the 2h compressive strength, 3d compressive strength and 3d positive tensile bond strength of each portion of the concrete thin layer repair materials were tested. According to GB / T 50080-2001 "Standard for Test Methods for Properties of Ordinary Concrete Mixtures", the test results shown in Table 1 below were obtained:
[0129] Table 1: Test results of concrete thin layer repair materials obtained in various implementation methods
[0130]
[0131] By comparing Example 1 with Comparative Example 5 in Table 1 above, it can be clearly seen that after the modified composite fiber is introduced into the present invention, the basic strength of the concrete is greatly improved. At the same time, Comparative Examples 1-4 are provided in the present invention to respectively verify that the pretreatment of carbon nanotubes, the pretreatment of polyethylene and polypropylene (including treatment with hexadecyltrimethylammonium bromide, blending of methylcellulose and ammonium bicarbonate, and immersion of the composite fiber in ammonia water) can improve the prepared concrete thin layer repair material in 2h compressive strength, 3d compressive strength and 3d positive tensile bonding strength, and can meet the demand for high-performance concrete thin layer repair materials.
[0132] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A concrete thin layer repair material, characterized in that: The following components are included by mass: Component A: 280-320 parts of sulphoaluminate cement, 30-70 parts of silicate cement, 5-35 parts of high-performance expansion agent, 30-70 parts of admixture, 550-600 parts of fine aggregate, 0.2-0.6 parts of polycarboxylate water reducer and 0.5-2 parts of retarder; Component B: 300-400 parts of water, 30-60 parts of modified composite fiber, 0.5-2 parts of inorganic dispersant, 0.2-1 parts of defoamer, 0.1-0.5 parts of wetting agent, 0.5-2 parts of antifreeze agent, 3-10 parts of nano silver antibacterial powder, 20-70 parts of water-based inorganic resin, 5-10 parts of lithium silicate, 5-10 parts of potassium silicate, 3-10 parts of redispersible latex powder and 0.2-1 parts of thickener; The modified composite fiber is prepared by the following method: S101, grinding polypropylene particles and polyethylene particles into powder to obtain polyethylene powder and polypropylene powder respectively, uniformly dispersing the polyethylene powder and polypropylene powder in a 2 mol / L hexadecyltrimethylammonium bromide solution and soaking them for 0.5-2 h, filtering after soaking, washing with deionized water, and vacuum drying at room temperature to obtain a mixed powder; S102, blending the mixed powder obtained in step S101 with methyl cellulose and ammonium bicarbonate respectively and stirring them evenly, melting the blended mixture, and stretching it in an extruder to form a composite fiber; S103, soaking the composite fiber obtained in step S102 in 25% ammonia water for 1-2 hours and then drying, dispersing the dried product in acetone, adding the modified carbon nanotubes and blending for 2-4 hours, then adding bisphenol A epoxy resin and heating and blending for 0.5-3 hours at a heating temperature of 40-80° C., filtering and drying to obtain the modified composite fiber; In step S102, the mass ratio of ammonium bicarbonate, methyl cellulose and mixed powder is 1:(1-3):(10-20); The mass ratio of the sum of the mass of the polypropylene particles and the polyethylene particles in step S101 to the mass of the modified carbon nanotubes, bisphenol A epoxy resin, acetone and ammonia water in step S103 is 1:(0.1-0.2):(0.4-0.5):(3-4):(8-12); The modified carbon nanotubes in step S103 are prepared by the following steps: S201, dispersing the carbon nanotubes into a mixed solution of sodium hydroxide and sodium dodecyl sulfate and soaking for 1-3 hours to obtain a mixed solution, wherein the molar concentration of the sodium hydroxide is 3 mol / L, and the concentration of the sodium dodecyl sulfate is 1 mol / L; S202, filtering the mixed solution added with carbon nanotubes in step S201, washing the filtered product with deionized water, and then calcining it in a muffle furnace at a temperature of 400-550°C for 2-5 hours to obtain modified carbon nanotubes.
2. A concrete thin layer repair material according to claim 1, characterized in that: In the step S101, the mass ratio of the polypropylene powder to the polyethylene powder is 1:(1-3), and the mass ratio of the sum of the mass of the polypropylene particles and the polyethylene particles to the hexadecyltrimethylammonium bromide solution is 1:(5-15).
3. A concrete thin layer repair material according to claim 1, characterized in that: The water-based inorganic resin is a water-based inorganic special resin of model E777-4, the inorganic dispersant is a silicate coating dispersant of model DISPERSOGEN SPS, the thickener is a polyurethane thickener of model AMS-201, the redispersible latex powder is a redispersible latex powder of model ZN-800T, and the wetting agent is a wetting agent of model KMT-7055.
4. A concrete thin layer repair material according to claim 1, characterized in that: The admixture is one of fly ash, slag powder, and silica ash, the fine aggregate is river sand with a particle size of 1-5 mm, the antifreeze is one of sodium nitrite, calcium chloride, and sodium chloride, the retarder is one of tartaric acid, potassium sodium tartrate, boric acid, borax, citric acid, and sodium gluconate, the high-performance expansion agent is one of calcium expansion agent and calcium-magnesium composite expansion agent, the modulus of the lithium silicate is 3.6-4.0, and the modulus of the potassium silicate is 2.5-3.
0.
5. The concrete thin layer repair material according to claim 1, characterized in that: In the step S201, the mass ratio of the carbon nanotubes to the mass ratio of the mixed solution of sodium hydroxide and sodium dodecyl sulfate is 1:
8.
6. A process for preparing a concrete thin layer repair material according to any one of claims 1 to 5, characterized in that: Use the following steps: S1. Add sulphoaluminate cement, silicate cement, high-performance expansion agent, admixture, fine aggregate, polycarboxylate water reducer and retarder to mixer A in proportion, stir and mix evenly to obtain component A of concrete thin layer repair material; S2, adding water, wetting agent, inorganic dispersant, defoamer, antifreeze agent and modified composite fiber to mixer B in proportion, with a stirring speed of 1300 r / min and a stirring time of 15 minutes; S3, continue to add nano silver antibacterial powder into mixer B in proportion, stirring at a speed of 1300 r / min, and stir for 15 minutes; S4, continue to add water-based inorganic resin, lithium silicate and potassium silicate into mixer B in proportion, stirring at a speed of 300 r / min for 15 minutes; S5. Continue to add the redispersed latex powder into the mixer B in proportion, stirring at a speed of 300 r / min for 10 minutes; S6. Continue to add thickener to mixer B in proportion at a stirring speed of 300 r / min, and stir for 10 minutes to obtain component B of concrete thin layer repair material; S7, adding the concrete thin layer repair material component B obtained in step S6 to the concrete thin layer repair material component A obtained in step S1, and continue to stir evenly to obtain the concrete thin layer repair material.
Citation Information
Patent Citations
Anti-crack concrete and preparation method thereof
CN112028557A
Preparation method of high-durability carbon nanotube modified fiber reinforced composite material
CN115418078A