An antioxidant high-temperature microwave absorbing material and its preparation method
By preparing LaxSr2-xMgMoO6-δ material, the problems of poor oxidation resistance and insufficient electromagnetic wave absorption performance at high temperature were solved, realizing the preparation and application of lightweight, oxidation-resistant high-temperature electromagnetic wave absorbing materials.
Patent Information
- Application Number
- CN202410721166.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-05
AI Technical Summary
Existing microwave absorbing materials have poor oxidation resistance at high temperatures, poor electromagnetic wave absorption performance, high preparation cost, complex process and low yield, and high density, making them unsuitable for large-scale production.
LaxSr2-xMgMoO6-δ was used as an antioxidant high-temperature microwave absorbing material. It was prepared by high-temperature solid-state synthesis using La2O3, SrCO3, MgO and MoO3 as raw powders. The powders were ball-milled, dried, and a binder was added before sintering to form a dense ceramic sheet.
The prepared LaxSr2-xMgMoO6-δ material exhibits good oxidation resistance and electromagnetic wave absorption performance at high temperatures, has low density, and is simple to prepare and can be mass-produced, making it suitable for large-scale applications.
Smart Images

Figure CN118598640B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of microwave absorbing materials technology, specifically relating to an antioxidant high-temperature microwave absorbing material and its preparation method. Background Technology
[0002] In recent years, due to the rapid development of the information age, reducing the probability of weapons being detected by the enemy in weaponized warfare has become an urgent problem to be solved, which has greatly promoted the development of stealth materials. Radar absorbing materials are special functional materials that can reduce the radar signature of a target (such as radar cross section (RCS)). By reducing the target's echo signal, enemy detectors cannot accurately locate the target in real time based on the echo signal.
[0003] When electromagnetic waves strike a material surface, some are reflected, some propagate through the material, and some are absorbed. Therefore, the impedance of the material needs to be matched as closely as possible to the impedance of the surrounding medium to reduce the reflectivity of the electromagnetic waves and allow as much of the wave as possible to enter the material. On the other hand, the electromagnetic waves entering the material should be attenuated and converted into other forms of energy as quickly and efficiently as possible. These are the two characteristics that microwave absorbing materials need to possess.
[0004] Current research on room-temperature electromagnetic wave absorbing materials is extensive, primarily focusing on carbon materials and ferrites, but also including other ceramic absorbing materials such as cobaltates (LaCoO3, etc.) and manganates (LaMnO3, CaMnO3, etc.). Carbon materials possess high conductivity and strong electrical losses, while ferrites also attenuate electromagnetic waves through magnetic losses. However, these materials are oxidized or demagnetized at high temperatures (>700K) (demagnetization targets inherently magnetic materials), or their conductivity increases, leading to impedance mismatch and the skin effect. Additionally, there are some high-temperature absorbing materials, such as zirconium boride (ZrB2), titanium boride (TiB2), and titanium nitride (TiN). While these materials exhibit some oxidation resistance, their manufacturing processes are complex, costly, and yield-low, making them unsuitable for large-scale production. Therefore, microwave absorbing materials composed entirely of oxides, possessing good oxidation resistance and maintaining electromagnetic wave absorption capabilities at high temperatures, are irreplaceable. However, some oxide ceramics have high densities; for example, LaCoO3 has a theoretical density of 7.29 g / cm³. 3 Therefore, it is not conducive to practical application.
[0005] Chinese patent application CN116904960A discloses a core-shell structured high-temperature absorbing material, its preparation method, and its application. This method uses reduced graphene oxide, trimethylaluminum, and deionized water as raw materials. Aluminum oxide is coated onto the surface of reduced graphene oxide using atomic layer deposition (ALD), forming an alumina-coated graphene core-shell structure. The thickness of the alumina coating is adjusted by precisely controlling the deposition rate, pulse time, and cycle number, thereby regulating the material's reflection loss. However, the ALD material preparation method has stringent requirements for precursor materials, a slow deposition rate, and is unsuitable for large-scale production. Furthermore, despite the alumina coating, TG curve observation shows that the material begins to decompose at 580℃ and completes decomposition at 650℃, indicating poor high-temperature resistance and oxidation resistance.
[0006] Chinese patent application CN115628646A discloses a high-temperature resistant radar absorbing material and a method for preparing an absorbing coating using this material, as well as its application. The method uses SrCO3 or Sr(NO3)2 as the Sr source and Ln2O3, Ln2(CO3)3, or Ln(NO3)3 as the Ln source, and SiO2 as the Si source. The ratio of Sr source to Ln source to Si source is (2-x):x:1. The absorber is prepared by ball milling, drying, and calcination. 2-x Ln x SiO4, where Ln is any lanthanide element. An absorbing coating is obtained through a spraying and curing process. The dielectric constant is adjusted by changing the doping amount of the lanthanide element, achieving electromagnetic wave absorption at high temperatures. However, in this patent, the real part of the dielectric constant is in the range of 11-18 at 900℃, while the imaginary part is only in the range of 0.1-0.7, indicating a small loss angle. This suggests that the material does not experience strong electromagnetic wave loss at high temperatures. The lowest reflection loss measured in the final test, only -3.5dB, meaning a plane electromagnetic wave absorption rate of only 65.4%, further confirms this.
[0007] Therefore, exploring a new antioxidant high-temperature absorbing agent is of great significance. Summary of the Invention
[0008] The purpose of this invention is to address the shortcomings of existing microwave absorbing materials, such as poor oxidation resistance at high temperatures, suboptimal electromagnetic wave absorption performance at high temperatures, high manufacturing costs, complex manufacturing processes, low yields, and high densities. The invention provides an oxidation-resistant high-temperature microwave absorbing material and its preparation method, which has the advantages of being lightweight and resistant to high-temperature oxidation.
[0009] The concept of this invention:
[0010] Based on the aforementioned objectives and the demand for antioxidant high-temperature microwave absorbing materials, this invention has conducted in-depth research. During the preliminary investigation, Sr2MgMoO was found to be... 6-δ Under reducing conditions, due to Mo5+ / Mo 6+ The increased electronic conductivity due to the increase in redox ion pairs and the increased ionic conductivity due to the increase in oxygen vacancies allow the material to achieve a conductivity of 8.60 S / cm at 800℃ and remain stable at temperatures as high as 1200℃. Furthermore, La has been found to be suitable for use in solid oxide fuel cells. x Sr 2-x MgMoO 6-δ It possesses high electrical conductivity and good thermal stability at high temperatures. Furthermore, Mg has a relatively small atomic mass and is one of the lightest metallic elements capable of forming high-temperature resistant dense oxides. Therefore, this invention considers La... x Sr 2-x MgMoO 6-δ (where x = 0 - 0.1) is very likely to become a potential antioxidant high-temperature absorbent, and this has been verified.
[0011] To achieve the above objectives, the technical solution provided by this invention is as follows:
[0012] La x Sr 2-x MgMoO 6-δ In the application of antioxidant high-temperature microwave absorbing materials, the value of x is 0-0.1.
[0013] A type of antioxidant high-temperature absorbing ceramic, unique in that its composition is La. x Sr 2-x MgMoO 6-δ , where x takes values from 0 to 0.1.
[0014] The preparation method of the above-mentioned antioxidant high-temperature absorbing ceramic is characterized by including the following steps:
[0015] 1) Weigh La2O3, SrCO3, MgO and MoO3 according to the stoichiometric ratio in the molecular formula, put them into a ball mill jar, and ball mill them to form a slurry using anhydrous ethanol as the solvent. The anhydrous ethanol can also be replaced with deionized water, but considering the subsequent drying steps, it is best to use volatile anhydrous ethanol as the solvent to reduce time costs.
[0016] 2) Dry the slurry obtained in step 1) to form ceramic powder;
[0017] 3) After grinding the ceramic powder obtained in step 2) evenly, take a portion of the ceramic powder, add the binder, and grind it evenly again.
[0018] 4) After pouring the uniform ceramic powder with binder added in step 3) into a mold and pressing it into a green body, embed it in the uniform ceramic powder without binder added in step 3), and sinter it in air atmosphere to obtain La. x Sr 2-x MgMoO 6-δ Ceramics. Since the high-temperature dielectric constant testing equipment (waveguide method) requires cuboid samples, it is best to choose a cuboid mold when making test samples using this method; for other types, the model can be designed according to the requirements.
[0019] Furthermore, in step 1), before weighing, La2O3 and MgO are annealed at 800-900℃ for 10-12 hours to remove carbonates and moisture, so that subsequent weighing and batching are accurate.
[0020] Further, in step 1), the weighed raw material is placed in a nylon ball mill, and anhydrous ethanol is used as the solvent. The material is then ball-milled using a planetary ball mill at a speed of 350-370 r / min for 12-16 h.
[0021] Furthermore, step 2) specifically involves:
[0022] Pour the slurry obtained in step 1) into a petri dish and place it on a heating table at 60-80℃ to dry for 10-12 hours to form ceramic powder.
[0023] Further, in step 3), the binder is a PVA solution with a mass fraction of 5%, and the mass ratio of ceramic powder to PVA solution is 30:1-40:1.
[0024] Further, in step 4), a tablet press is used to press the tablet into a blank, with a pressure of 18-20 MPa and a time of 5-10 min;
[0025] The sintering process is as follows: pre-fire at 400-500℃ for 2-4 hours in a muffle furnace with an air atmosphere, and then sinter at 1200-1350℃ for 28-30 hours. The purpose of the low-temperature pre-firing at 400-500℃ is because PVA binder was used in the aforementioned process. Low-temperature pre-firing removes the binder, which helps to improve the density of the ceramic material at high temperature, resulting in better material contact and increased electrical conductivity loss.
[0026] In addition, the present invention also provides a device with radar stealth function, which uses the above-mentioned antioxidant high-temperature absorbing material as a filler.
[0027] The principle of this invention:
[0028] This invention uses La2O3, SrCO3, MgO, and MoO3 as raw materials to prepare La via a high-temperature solid-state synthesis method. x Sr2-x MgMoO 6-δ , where x = 0 - 0.1.
[0029] For materials where x > 0, on the one hand, La 3+ The ionic radius of Sr is 0.136 nm. 2+ The ionic radius is 0.144 nm, and the difference between the two ionic radii is small. Therefore, La 3+ A small amount of substitution has little effect on lattice distortion, thus resulting in high crystal structure stability. This high structural stability contributes to the material's high-temperature thermal stability, i.e., its resistance to oxidation and high-temperature absorption. On the other hand, La... 3+ Replace Sr 2+ The position makes Mo 6+ The valence state decreases to Mo 5+ Increased electrical conductivity in materials leads to enhanced electromagnetic wave conductance loss (heterovalent substitution significantly improves conductivity than homovalent substitution, or in other words, heterovalent substitution provides a greater performance improvement); therefore, research on La... x Sr 2-x MgMoO 6-δ The oxidation resistance and high-temperature wave absorption capacity of the material are of great significance.
[0030] Meanwhile, this invention also confirms this new application; the La prepared by this invention... x Sr 2-x MgMoO 6-δ The sheet has a density of 90%-92%, forming a good conductive path, but exhibiting some conductivity loss at high temperatures. On the other hand, due to intense ion vibrations at high temperatures, oxygen ions on the crystal lattice have sufficient energy to break free from their lattice constraints, creating oxygen vacancies. Since these oxygen vacancies carry two units of positive charge, the ionic conductivity of the material increases. To achieve chemical valence equilibrium, the Mo inside the material... 6+ The valence state of Mo will decrease, causing Mo to 5+ / Mo 6+ The increase in redox ion pairs further increases the electronic conductivity of the material, thus improving the La... x Sr 2-x MgMoO 6-δ The material exhibits strong dielectric loss at high temperatures, thereby achieving strong loss of electromagnetic waves at high temperatures.
[0031] The advantages of this invention are:
[0032] This invention relates to anti-oxidation high-temperature absorbing ceramic La x Sr 2-x MgMoO 6-δThe raw materials used are inexpensive and readily available, the entire preparation process is simple, and it can be produced in large quantities. Furthermore, Mg is one of the lightest metallic elements capable of forming high-temperature resistant dense oxides, and the resulting La... x Sr 2-x MgMoO 6-δ (x = 0 - 0.1) The density of the material is 4.9 - 5.1 g / cm³. 3 La is a lightweight electromagnetic wave absorbing material. Compared to existing electromagnetic wave absorbing materials, the La prepared in this invention... x Sr 2-x MgMoO 6-δ The phase did not decompose after being held at 800℃ for 2 hours (if the phase decomposes after high-temperature annealing, it is generally due to the increase of phases, and the high-temperature stability of the material can be analyzed from the XRD diagram). It has good oxidation resistance and good attenuation characteristics at high temperatures. It is an oxidation-resistant high-temperature electromagnetic wave absorbing material from room temperature to 800℃. Attached Figure Description
[0033] Figure 1 This is a flowchart illustrating the preparation process of the present invention.
[0034] Figure 2 The images are XRD patterns after annealing at 800°C for 2 hours in Examples 2, 3, and 6.
[0035] Figure 3 The diagram shows the real part of the dielectric constant in the x-band at 200°C in Examples 1, 4, and 7.
[0036] Figure 4 The diagram shows the imaginary part of the dielectric constant in the x-band at 200°C in Examples 1, 4, and 7.
[0037] Figure 5 La prepared in Example 1 x Sr2MgMoO 6-δ (x=0) Reflection loss curves of ceramic sheets at different thicknesses at 600℃. Detailed Implementation
[0038] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments:
[0039] The pharmaceutical raw materials, instruments, and equipment used in this invention can all be purchased on the market.
[0040] The molar mass of SrCO3 is 147.63 g / mol, the specification is analytical grade, the form is white powder, and the manufacturer is Sinopharm Chemical Reagent Co., Ltd.
[0041] The molar mass of Sr(NO3)2 is 211.63 g / mol, the specification is analytical grade, the form is white powder, and the manufacturer is Sinopharm Chemical Reagent Co., Ltd.
[0042] The molar mass of MgO is 40.3 g / mol, the specification is analytical grade, the form is white powder, and the manufacturer is Tianjin Fuchen Chemical Reagent Factory.
[0043] The molar mass of MoO3 is 143.94 g / mol, the specification is analytical grade, the form is gray-green powder, and the manufacturer is Shanghai Maclean Biochemical Technology Co., Ltd.
[0044] The molar mass of La2O3 is 325.84 g / mol, the specification is analytical grade, the form is white powder, and the manufacturer is Shanghai Aladdin Biochemical Technology Co., Ltd.
[0045] The molar mass of anhydrous ethanol is 46.07 g / mol, the specification is analytical grade, the form is transparent liquid, and the manufacturer is Guangdong Guanghua Technology Co., Ltd.
[0046] Muffle furnace model: KSL-1200X, manufacturer: Hefei Kejing Materials Technology Co., Ltd.
[0047] The ball mill model is YXQM-4L, and the manufacturer is Changsha Miqi Instrument Equipment Co., Ltd.
[0048] Example 1: La x Sr 2-x MgMoO 6-δ Preparation of (x=0)
[0049] Step 1: Annealing and impurity removal
[0050] 10g of raw MgO powder was annealed in a muffle furnace at 800℃ for 12h to remove carbonates and moisture, ensuring accurate weighing and batching in the future.
[0051] Step 2: Mix the ingredients
[0052] Based on the molecular formula Sr2MgMoO 6-δ The calculated stoichiometric ratio was determined according to Sr∶Mg∶Mo=2∶1∶1. 37.7093g SrCO3, 5.1469g MgO, and 18.3847g MoO3 were weighed and mixed in a ball mill jar with 160ml anhydrous ethanol as the solvent.
[0053] Step 3: Ball milling
[0054] The planetary ball mill was set to a speed of 350 r / min and a milling time of 16 h to obtain a uniformly mixed slurry.
[0055] Step 4: Drying
[0056] The ball-milled slurry was poured into a petri dish and dried on a 60°C electric heating plate for 12 hours to form ceramic powder.
[0057] Step 5: Add adhesive
[0058] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder according to the ceramic powder to PVA solution mass ratio of 30:1, add 0.1497g of 5% PVA solution, and continue grinding evenly.
[0059] Step 6: Pressing the blank
[0060] The treated ceramic powder is poured into a mold, and the mold is placed on a pressing table. The pressure of the pressing machine is 18 MPa and the time is 5 minutes to press the ceramic powder into a green body for subsequent sintering.
[0061] Step 7: Sintering
[0062] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 400℃ for 4 hours in air atmosphere, then sinter it at 1200℃ for 28 hours to obtain Sr2MgMoO. 6-δ Ceramic shards.
[0063] Step 8: Grinding and polishing
[0064] For ease of testing, the sintered Sr2MgMoO 6-δ The ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was 120 grit. The dimensions of the polished ceramic sheet were set to 22.90 mm in length, 10.2 mm in width, and 1.02 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0065] Example 2: La x Sr 2-x MgMoO 6-δ (x = 0.02)
[0066] Step 1: Annealing and impurity removal
[0067] 10g of MgO and 10g of La2O3 raw powder were annealed in a muffle furnace at 900℃ for 12h to remove carbonates and moisture, so as to ensure accurate subsequent weighing and batching.
[0068] Step 2: Mix the ingredients
[0069] Through the molecular formula La0.02 Sr 1.98 MgMoO 6-δ The calculated stoichiometric ratio was La∶Sr∶Mg∶Mo=0.02∶1.98∶1∶1. 0.3396g La2O3, 30.4610g SrCO3, 4.1996g MgO, and 14.9998g MoO3 were weighed and mixed in a ball mill jar with 130ml anhydrous ethanol as the solvent.
[0070] Step 3: Ball milling
[0071] The planetary ball mill was set to a speed of 370 r / min and a milling time of 12 h to obtain a uniformly mixed slurry.
[0072] Step 4: Drying
[0073] The ball-milled slurry was poured into a petri dish and dried on a 70°C electric heating plate for 11 hours to form ceramic powder.
[0074] Step 5: Add adhesive
[0075] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder according to the ceramic powder to PVA solution mass ratio of 32:1, add 0.1407g of 5% PVA solution, and continue grinding evenly.
[0076] Step 6: Pressing the blank
[0077] The treated ceramic powder is poured into a mold, and the mold is placed on a pressing table. The pressure of the pressing machine is 20 MPa and the time is 7 minutes to press the ceramic powder into a green body for subsequent sintering.
[0078] Step 7: Sintering
[0079] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 500℃ for 2 hours in air atmosphere, then sinter it at 1300℃ for 30 hours to obtain La. 0.02 Sr 1.98 MgMoO 6-δ Ceramic shards.
[0080] Step 8: Grinding and polishing
[0081] For ease of testing, the sintered La 0.02 Sr 1.98 MgMoO 6-δThe ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was 120 grit. The dimensions of the polished ceramic sheet were set to 23.01 mm in length, 10.24 mm in width, and 1.56 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0082] Example 3: La x Sr 2-x MgMoO 6-δ (x = 0.04)
[0083] Step 1: Annealing and impurity removal
[0084] 10g of MgO and 10g of La2O3 raw powder were annealed in a muffle furnace at 900℃ for 12h to remove carbonates and moisture, so as to ensure accurate subsequent weighing and batching.
[0085] Step 2: Mix the ingredients
[0086] Through the molecular formula La 0.04 Sr 1.96 MgMoO 6-δ The calculated stoichiometric ratio was La∶Sr∶Mg∶Mo=0.04∶1.96∶1∶1. 0.6787g La₂O₃, 30.1341g SrCO₃, 4.1969g MgO, and 14.9903g MoO₃ were weighed and mixed in a ball mill jar with 130ml anhydrous ethanol as the solvent.
[0087] Step 3: Ball milling
[0088] The planetary ball mill was set to a speed of 370 r / min and a milling time of 12 h to obtain a uniformly mixed slurry.
[0089] Step 4: Drying
[0090] The ball-milled slurry was poured into a petri dish and dried on an electric heating table at 80°C for 10 hours to form ceramic powder.
[0091] Step 5: Add adhesive
[0092] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder according to the ceramic powder to PVA solution mass ratio of 34:1, add 0.1322g of 5% PVA solution, and continue grinding evenly.
[0093] Step 6: Pressing the blank
[0094] The treated ceramic powder is poured into a mold, and the mold is placed on a pressing table. The pressure of the pressing machine is 19 MPa and the time is 8 minutes to press the ceramic powder into a green body for subsequent sintering.
[0095] Step 7: Sintering
[0096] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 500℃ for 2 hours in air atmosphere, then sinter it at 1350℃ for 30 hours to obtain La. 0.04 Sr 1.96 MgMoO 6-δ Ceramic shards.
[0097] Step 8: Grinding and polishing
[0098] For ease of testing, the sintered La 0.04 Sr 1.96 MgMoO 6-δ The ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was 120 grit. The dimensions of the polished ceramic sheet were set to 23.03 mm in length, 10.23 mm in width, and 1.64 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0099] Example 4: La x Sr 2-x MgMoO 6-δ (x = 0.05)
[0100] Step 1: Annealing and impurity removal
[0101] 10g of MgO and 10g of La2O3 raw powder were annealed in a muffle furnace at 900℃ for 12h to remove carbonates and moisture, so as to ensure accurate subsequent weighing and batching.
[0102] Step 2: Mix the ingredients
[0103] Through the molecular formula La 0.05 Sr 1.95 MgMoO 6-δ The calculated stoichiometric ratio was La∶Sr∶Mg∶Mo=0.05∶1.95∶1∶1. 0.8481g La2O3, 29.9708g SrCO3, 4.1956g MgO, and 14.9855g MoO3 were weighed and mixed in a ball mill jar with 130ml anhydrous ethanol as the solvent.
[0104] Step 3: Ball milling
[0105] The planetary ball mill was set to a speed of 356 r / min and a milling time of 15 h to obtain a uniformly mixed slurry.
[0106] Step 4: Drying
[0107] The ball-milled slurry was poured into a petri dish and dried on an electric heating table at 80°C for 10 hours to form ceramic powder.
[0108] Step 5: Add adhesive
[0109] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder according to the ceramic powder to PVA solution mass ratio of 36:1, add 0.1253g of 5% PVA solution, and continue grinding evenly.
[0110] Step 6: Pressing the blank
[0111] The treated ceramic powder is poured into a mold, the mold is placed on a pressing table, the pressure of the pressing machine is 20MPa, and the time is 10min, the ceramic powder is pressed into a green body for subsequent sintering.
[0112] Step 7: Sintering
[0113] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 500℃ for 2 hours in air atmosphere, then sinter it at 1350℃ for 30 hours to obtain La. 0.05 Sr 1.95 MgMoO 6-δ Ceramic shards.
[0114] Step 8: Grinding and polishing
[0115] For ease of testing, the sintered La 0.05 Sr 1.95 MgMoO 6-δ The ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was 120 grit. The dimensions of the polished ceramic sheet were set to 22.96 mm in length, 10.19 mm in width, and 1.44 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0116] Example 5: La x Sr 2-x MgMoO 6-δ (x = 0.06)
[0117] Step 1: Annealing and impurity removal
[0118] 10g of MgO and 10g of La2O3 raw powder were annealed in a muffle furnace at 900℃ for 12h to remove carbonates and moisture, so as to ensure accurate subsequent weighing and batching.
[0119] Step 2: Mix the ingredients
[0120] Through the molecular formula La 0.05 Sr 1.95 MgMoO 6-δ The calculated stoichiometric ratio was La∶Sr∶Mg∶Mo=0.06∶1.94∶1∶1. 1.0174g La2O3, 29.8076g SrCO3, 4.1943g MgO, and 14.9807g MoO3 were weighed and mixed in a ball mill jar with 130ml anhydrous ethanol as the solvent.
[0121] Step 3: Ball milling
[0122] The planetary ball mill was set to a speed of 365 r / min and a milling time of 14 h to obtain a uniformly mixed slurry.
[0123] Step 4: Drying
[0124] The ball-milled slurry was poured into a petri dish and dried on an electric heating table at 80°C for 10 hours to form ceramic powder.
[0125] Step 5: Add adhesive
[0126] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder according to the ceramic powder to PVA solution mass ratio of 38:1, add 0.1186g of 5% PVA solution, and continue grinding evenly.
[0127] Step 6: Pressing the blank
[0128] The treated ceramic powder is poured into a mold, the mold is placed on a pressing table, the pressure of the pressing machine is 18MPa, and the time is 10min to press the ceramic powder into a green body for subsequent sintering.
[0129] Step 7: Sintering
[0130] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 500℃ for 2 hours in air atmosphere, then sinter it at 1350℃ for 30 hours to obtain La. 0.06 Sr 1.94 MgMoO 6-δ Ceramic shards.
[0131] Step 8: Grinding and polishing
[0132] For ease of testing, the sintered La 0.06 Sr 1.94 MgMoO 6-δ The ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was 120 grit. The dimensions of the polished ceramic sheet were set to 22.96 mm in length, 10.19 mm in width, and 1.44 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0133] Example 6: La x Sr 2-x MgMoO 6-δ (x = 0.08)
[0134] Step 1: Annealing and impurity removal
[0135] 10g of MgO and 10g of La2O3 raw powder were annealed in a muffle furnace at 900℃ for 12h to remove carbonates and moisture, so as to ensure accurate subsequent weighing and batching.
[0136] Step 2: Mix the ingredients
[0137] Through the molecular formula La 0.08 Sr 1.92 MgMoO 6-δ The calculated stoichiometric ratio was La∶Sr∶Mg∶Mo=0.08∶1.92∶1∶1. 1.3556g La2O3, 29.4816g SrCO3, 4.1916g MgO, and 14.9807g MoO3 were weighed and mixed in a ball mill jar with 130ml anhydrous ethanol as the solvent.
[0138] Step 3: Ball milling
[0139] The planetary ball mill was set to a speed of 370 r / min and a milling time of 12 h to obtain a uniformly mixed slurry.
[0140] Step 4: Drying
[0141] The ball-milled slurry was poured into a petri dish and dried on an electric heating table at 80°C for 10 hours to form ceramic powder.
[0142] Step 5: Add adhesive
[0143] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder and add 0.1135g of 5% PVA solution according to the ceramic powder to PVA solution mass ratio of 40:1, and continue grinding evenly.
[0144] Step 6: Pressing the blank
[0145] The treated ceramic powder is poured into a mold, and the mold is placed on a pressing table. The pressure of the pressing machine is 19 MPa and the time is 10 min to press the ceramic powder into a green body for subsequent sintering.
[0146] Step 7: Sintering
[0147] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 500℃ for 2 hours in air atmosphere, then sinter it at 1350℃ for 30 hours to obtain La. 0.08 Sr 1.92 MgMoO 6-δ Ceramic shards.
[0148] Step 8: Grinding and polishing
[0149] For ease of testing, the sintered La 0.08 Sr 1.92 MgMoO 6-δ The ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was 120 grit. The dimensions of the polished ceramic sheet were set to 23.02 mm in length, 10.18 mm in width, and 1.26 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0150] Example 7: La x Sr 2-x MgMoO 6-δ (x=0.1)
[0151] Step 1: Annealing and impurity removal
[0152] 10g of MgO and 10g of La2O3 raw powder were annealed in a muffle furnace at 900℃ for 12h to remove carbonates and moisture, so as to ensure accurate subsequent weighing and batching.
[0153] Step 2: Mix the ingredients
[0154] Through the molecular formula La 0.05 Sr 1.95 MgMoO 6-δ The calculated stoichiometric ratio was La∶Sr∶Mg∶Mo=0.1∶1.9∶1∶1. 1.6935g La2O3, 29.1559g SrCO3, 4.1889g MgO, and 14.9617g MoO3 were weighed and mixed in a ball mill jar with 130ml anhydrous ethanol as the solvent.
[0155] Step 3: Ball milling
[0156] The planetary ball mill was set to a speed of 368 r / min and a milling time of 13 h to obtain a uniformly mixed slurry.
[0157] Step 4: Drying
[0158] The ball-milled slurry was poured into a petri dish and dried on a 70°C electric heating plate for 11 hours to form ceramic powder.
[0159] Step 5: Add adhesive
[0160] After grinding the ceramic powder evenly in a mortar, weigh 4.5g of ceramic powder and add 0.1136g of 5% PVA solution according to the ceramic powder to PVA solution mass ratio of 40:1, and continue grinding evenly.
[0161] Step 6: Pressing the blank
[0162] The treated ceramic powder is poured into a mold, the mold is placed on a pressing table, the pressure of the pressing machine is 20MPa, and the time is 10min, the ceramic powder is pressed into a green body for subsequent sintering.
[0163] Step 7: Sintering
[0164] Take a small amount of ceramic powder from step 4, embed the green body obtained in step 6 into it, place it in a crucible, put the crucible in a muffle furnace, and calcine it at 500℃ for 2 hours in air atmosphere, then sinter it at 1350℃ for 30 hours to obtain La. 0.1 Sr 1.9 MgMoO 6-δ Ceramic shards.
[0165] Step 8: Grinding and polishing
[0166] For ease of testing, the sintered La 0.1 Sr 1.9 MgMoO 6-δ The ceramic sheet was placed on a polishing machine, held down with both hands. The polishing machine was set to 500 rpm, and the sandpaper was set to 120 grit. The dimensions of the polished ceramic sheet were set to 23.04 mm in length, 10.18 mm in width, and 1.68 mm in thickness. The polished ceramic sheet was then polished on 1000 grit sandpaper to obtain a dielectric sample for testing.
[0167] First, such as Figure 2 The La prepared in Examples 2, 3, and 6 are shown below. x Sr 2-x MgMoO 6-δThe materials (x = 0.02, 0.04, and 0.08) did not show new diffraction peaks in XRD after annealing at 800℃ for 2 hours in air, indicating that the material structure did not decompose and it possesses a certain degree of structural stability at high temperatures. Secondly, through the high-temperature dielectric constant, such as... Figure 3 and Figure 4 The analysis shown indicates that at 200℃, as La... 3+ With increasing doping content, both the real and imaginary parts of the dielectric constant of the material increase. The real part of the complex dielectric constant characterizes the material's ability to store charge, while the imaginary part represents its ability to dissipate electromagnetic waves. The increase in the real part indicates enhanced polarization capability, while the increase in the imaginary part is attributed to increased polarization relaxation loss and increased conductivity loss, indicating that with increasing La... 3+ Increased doping content leads to an increase in the concentration of oxygen vacancies within the material and Mo 5+ The increase in ion concentration enhances the material's conductivity loss and its ability to dissipate electromagnetic waves. Example 7 exhibits the strongest electromagnetic wave dissipation capability, thus proving that La... x Sr 2- x MgMoO 6-δ It can be used as a high-temperature absorbing material for electromagnetic wave anti-oxidation. For example... Figure 5 As shown, the reflection loss of Example 1 at 600°C was calculated, and it was found that La x Sr 2-x MgMoO 6-δ (x=0) The ceramic with a thickness of 1.5mm at 600℃ has a maximum effective bandwidth of 1.86GHz (RL value < -10dB), La x Sr 2-x MgMoO 6-δ (x=0) The ceramic thickness of 1.4mm has the minimum reflection loss: -28.356dB, further demonstrating that La x Sr 2-x MgMoO 6-δ (x=0) Ceramics exhibit certain impedance matching and attenuation loss characteristics at 600℃. La... x Sr 2-x MgMoO 6-δ (When x>0) The high dielectric constant and oxidation resistance at high temperatures also confirm that it can be used as an anti-oxidation high-temperature absorbing material. Whether it is the aforementioned microwave absorbing ceramic or as a filler mixed with a microwave-transparent matrix to form a high-temperature anti-oxidation electromagnetic wave absorbing material, it can provide theoretical support for the subsequent application of high-temperature microwave absorbing coatings. In addition, the high dielectric constant is also conducive to reducing the material thickness, which is very important for microwave absorbing materials.
[0168] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the scope of the technology disclosed in the present invention, and such modifications or substitutions should all be covered within the scope of protection of the present invention.
Claims
1. La x Sr 2-x MgMoO 6-δ As an application of antioxidant high-temperature absorbing materials, among which, The value of x is 0-0.
1.
2. A device with radar stealth capability, characterized in that: It uses La x Sr 2-x MgMoO 6-δ Antioxidant high-temperature absorbing material is used as a filler for absorbing waves, where the value of x is 0-0.1.
Citation Information
Patent Citations
High-temperature-resistant radar wave-absorbing material as well as method for preparing wave-absorbing coating by using material and application of high-temperature-resistant radar wave-absorbing material
CN115628646A
High-temperature-resistant wave-absorbing material with core-shell structure as well as preparation method and application thereof
CN116904960A
Densification method of Sr2MgMoO6 type cell anode material
CN102044680A
Method for preparing stable double perovskite type Sr2-xAxMg1-yByMoO6 anode material in air atmosphere
CN103378363A