A peroxide cross-linked polyethylene insulation material and preparation method thereof
By introducing modified nanosepiolite into polyethylene insulating material, a network crosslinking structure is formed, and the cyclopentadiene and hexene structures are used to depolymerize and absorb heat at high temperatures, the silane crosslinking polyethylene cable material is solved at high temperatures. The problem of poor aging resistance has achieved higher high-temperature aging resistance.
Patent Information
- Application Number
- CN202410950543.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Existing silane crosslinked polyethylene cable materials have poor aging resistance at high temperatures, which limits the use of high temperature requirements such as wind energy cables and photovoltaic cables.
By introducing modified nanosepiolite, a network crosslinked structure is formed, and the cyclopentadiene and hexene structures are used to depolymerize and absorb heat at high temperatures, protect the polyethylene material from free radical attacks, and improve the high-temperature aging resistance.
It significantly improves the high-temperature aging resistance of polyethylene insulating materials, meets the high-temperature operation requirements of 170℃ and above, and extends the service life of the cable.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of cable materials, in particular to a peroxide cross-linked polyethylene insulating material and a preparation method thereof. Background Art
[0002] The development of electric energy is related to the national economy, people's livelihood and national security. With the sustained and rapid development of my country's economy and society, the demand for electricity has also entered a period of rapid growth. By the end of 2016, the total electricity consumption of the whole society reached 5.92 trillion kW·h, and it is expected that the total electricity consumption of the whole society will reach 68,000~7.2 trillion kW·h in 2020. Due to the reverse distribution characteristics of my country's energy base and power load center, higher requirements are put forward for the construction of the power system. It is necessary to develop ultra-high voltage, long-distance, large-capacity and low-loss power networks to help the national development plan, and high-voltage direct current transmission technology is an effective way to solve this problem.
[0003] The earliest DC transmission project can be traced back to 1882, when Germany used a single DC generator to generate electricity and transmitted electricity to the International Exhibition in Munich through a 57 km overhead line. In the early stages of development, DC transmission was relatively backward due to technical difficulties such as the complex operation of DC motors in series. With the development of electronic and electrical technology, the economy and stability of high-voltage DC transmission technology began to emerge, and high-voltage DC transmission projects have developed rapidly. As an important part of high-voltage DC transmission, high-voltage DC cable transmission has the advantages of small footprint, little impact from environmental pollution and climatic conditions, high transmission stability, and small workload for daily operation and maintenance.
[0004] According to the different insulating media, high-voltage DC cables can be divided into oil-filled cables, viscous impregnated paper cables and plastic insulated cables. Plastic insulated cables have the advantages of light weight, simple operation and maintenance, and good insulation performance, and are widely used in low, medium and high voltage cable insulation. At present, cross-linked polyethylene (XLPE) is used as the main cable insulation for high-voltage DC plastic cables. XLPE maintains the advantages of high insulation resistance, good voltage resistance, low dielectric constant and dielectric loss of polyethylene, and has better thermal and mechanical properties than polyethylene, and its comprehensive performance is significantly improved. However, with the large-scale use of XLPE as a cable insulation material, many problems and technical difficulties in the production, operation and recycling of XLPE cables have gradually emerged. How to maximize the performance of XLPE cables to ensure the safety and stability of cable operation has always been the most concerned and urgent key issue in the academic and engineering fields.
[0005] At present, the long-term operating temperature of silane cross-linked polyethylene cable materials on the market is only 90°C. For cables with higher temperature resistance requirements, such as wind power cables, photovoltaic cables, equipment cables, etc., the application of ordinary silane cross-linked polyethylene cable materials is limited. Summary of the invention
[0006] In order to overcome the problem of poor high temperature aging resistance of wire and cable materials due to the introduction of water molecules by silane crosslinking, a peroxide cross-linked polyethylene insulation material is provided. By introducing modified nano-sepiolite, a network cross-linked structure is formed at room temperature. At high temperature, it depolymerizes to form cyclopentadiene to absorb high temperature energy, thereby alleviating the aging risk of polyethylene.
[0007] A peroxide cross-linked polyethylene insulating material comprises the following raw materials by weight: 20-35 parts of high-density polyethylene, 20-30 parts of linear low-density polyethylene, 1-5 parts of modified sepiolite, 0.5-2.1 parts of a peroxide cross-linking agent, 0.1-1 parts of a co-cross-linking agent and 0.5-15 parts of a functional additive; wherein cyclopentadienoic acid and hexenoic acid are grafted on the surface of the modified sepiolite.
[0008] In some embodiments of the present invention, the method for preparing the modified sepiolite comprises the following steps:
[0009] S1: Mix the nano-sepiolite and the acid solution in a solid-liquid ratio of 1-3 g: 10-16 ml, stir to fully react, centrifuge, filter, and wash until the pH of the final filtrate is neutral, and dry the obtained acid-treated nano-sepiolite for standby use;
[0010] S2: Mix cyclopentadienoic acid, hexenoic acid and the acid-treated nano-sepiolite obtained in S1, drop concentrated sulfuric acid therein, heat under reflux to start the reaction, wait for the reaction to be completed, cool to room temperature, filter, dry and grind to obtain the modified sepiolite.
[0011] Furthermore, the concentration of the acid solution in S1 is 1-2 mol / L, and the type is at least one of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid.
[0012] Furthermore, the cyclopentadienoic acid in S2 is at least one of 2,4-cyclopentadiene-1-acetic acid and 2,4-cyclopentadiene-1-carboxylic acid.
[0013] Further, the liquid-to-solid ratio of the cyclopentadienoic acid, hexenoic acid and the acid-treated nano-sepiolite obtained in S2 is 5-8 ml: 10-17 ml: 2-5 g. Wherein, the hexenoic acid is at least one of cis-3-hexenoic acid and trans-3-hexenoic acid.
[0014] The modified nano sepiolite described in the present invention is prepared by esterification reaction of hydroxyl groups on the surface of nano sepiolite after acid treatment with carboxyl groups of cyclopentadienoic acid and hexenoic acid. Since the cyclopentadiene structure and the hexene structure can undergo Diels-Alder reaction at room temperature to form a dicyclopentadiene structure, when subjected to high temperature treatment of 170°C or above, the dicyclopentadiene structure can be depolymerized into cyclopentadiene and hexene structures. These two structures are combined with the porous structure of sepiolite to withstand the impact of high temperature heat, protecting the carbon-carbon single bond of polyethylene from the attack of free radicals. Therefore, the inventor introduces the modified nano sepiolite into the synthesis of polyethylene insulating material with the help of this characteristic, forms a mesh structure composed of dicyclopentadiene in the polyethylene cross-linked material, protects the polyethylene cross-linked material from the strong attack of free radicals, alleviates its high temperature aging degree, and improves its high temperature resistance grade.
[0015] Because the existence of free radicals or heat can make the cyclopentadiene structure homopolymerize, forming thermal irreversible permanent crosslinking. In order to avoid the occurrence of this situation, improve the thermal reversibility of the dicyclopentadiene crosslinked structure, the inventor found through experiments that when the liquid-solid ratio of the used cyclopentadienoic acid and hexenoic acid and acid-treated nano sepiolite is 5-8ml: 10-17ml: 2-5g, when the obtained modified nano sepiolite is used as a nano filler in a peroxide crosslinked polyethylene insulating material, the obtained peroxide polyethylene insulating material has better high temperature aging resistance.
[0016] In some embodiments of the present invention, the peroxide crosslinking agent is at least one of ethylene peroxide, monomethyl ether peroxide, and dicumyl peroxide.
[0017] In some embodiments of the present invention, the auxiliary cross-linking agent is at least one of triallyl cyanurate, triallyl isocyanurate, and propane trimethanol triacrylate.
[0018] In some embodiments of the present invention, the functional additive is at least one of a plasticizer, an antioxidant, and a lubricant. The plasticizer may be dibutyl phthalate, dioctyl phthalate, epoxy soybean oil, tricresyl phosphate, triphenyl phosphate, etc.; the antioxidant is at least one of a hydroxylated antioxidant, an alkyl biphenyl antioxidant, and a hydroxyphosphonate antioxidant; the lubricant is at least one of oleamide, erucamide, stearamide, and ethylene bisstearamide.
[0019] The method for preparing the above-mentioned peroxide cross-linked polyethylene insulation material comprises the following steps:
[0020] SS1: Mix all raw material components except the peroxide crosslinking agent according to the formula and put them into an internal mixer for melt blending at a mixing temperature of 120-150°C for 8-10 minutes to obtain a mixed material;
[0021] SS2: Add the mixed material into a twin-screw extruder and extrude it through four working zones to obtain pellets; wherein the working temperature of the first zone is 80-90°C, the working temperature of the second zone is 100-110°C, the working temperature of the third zone is 120-130°C, and the working temperature of the fourth zone is 120-130°C;
[0022] SS3: The peroxide cross-linking agent is heated and melted into a liquid for metering, and mixed with the pellets obtained in SS2 at 80-100°C to diffuse the peroxide cross-linking agent into the interior of the pellets, and then added to a single-screw extruder and extruded into wires through two zones, wherein the working temperature of the first zone is 80-90°C and the working temperature of the second zone is 100-120°C; peroxide cross-linked polyethylene insulation material is obtained.
[0023] Beneficial effects: Compared with the prior art, the peroxide cross-linked polyethylene insulating material provided by the present invention contains specially modified sepiolite as a nanofiller, and the cyclopentadiene structure and the hexene structure grafted on the surface of the modified sepiolite can undergo a Diels-Alder reaction at room temperature to form a cross-linked network structure of a dicyclopentadiene structure, thereby protecting the polyethylene material from aging caused by interference from external factors; more importantly, the dicyclopentadiene structure will depolymerize into cyclopentadiene and hexene at 170°C, and these two structures can consume free radicals in the polyethylene material, thereby protecting the carbon-carbon single bonds of the polyethylene, and finally the high-temperature aging resistance of the peroxide cross-linked polyethylene insulating material is enhanced. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0025] The following is an exemplary description of the preparation process of the modified sepiolite used in the examples. The nano sepiolite used was purchased from Xiangtan Yuanyuan Sepiolite Co., Ltd.:
[0026] Modified Sepiolite-1
[0027] S1: Mix the nano-sepiolite with 1 mol / L hydrochloric acid solution at a solid-liquid ratio of 1 g:10 ml, stir to fully react, centrifuge, filter, and wash until the pH of the final filtrate is neutral, and dry the obtained acid-treated nano-sepiolite for later use;
[0028] S2: 20 ml of 2,4-cyclopentadiene-1-acetic acid, 10 ml of cis-3-hexenoic acid and 4 g of the acid-treated nano-sepiolite obtained in S1 were mixed, concentrated sulfuric acid was dropped into the mixture, and the mixture was heated under reflux to start the reaction. The reaction was continued for 2 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, dried and ground to obtain the modified sepiolite-1.
[0029] Modified Sepiolite-2
[0030] S1: Mix the nano-sepiolite with a 1.5 mol / L sulfuric acid solution at a solid-liquid ratio of 2 g:13 ml, stir to fully react, centrifuge, filter, and wash until the pH of the final filtrate is neutral, and dry the resulting acid-treated nano-sepiolite for later use;
[0031] S2: 28 ml of 2,4-cyclopentadiene-1-acetic acid, 12 ml of trans-3-hexenoic acid and 6 g of the acid-treated nano-sepiolite obtained in S1 were mixed, concentrated sulfuric acid was dropped into the mixture, and the mixture was heated under reflux to start the reaction. The reaction lasted for 3 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, dried and ground to obtain the modified sepiolite-2.
[0032] Modified Sepiolite-3
[0033] S1: Mix the nano-sepiolite with a 2 mol / L nitric acid solution at a solid-liquid ratio of 3 g:16 ml, stir to fully react, centrifuge, filter, and wash until the pH of the final filtrate is neutral, and dry the resulting acid-treated nano-sepiolite for later use;
[0034] S2: 34 ml of 2,4-cyclopentadiene-1-carboxylic acid, 16 ml of cis-3-hexenoic acid and 10 g of the acid-treated nano-sepiolite obtained in S1 were mixed, concentrated sulfuric acid was dropped into the mixture, and the mixture was heated under reflux to start the reaction. The reaction lasted for 4 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, dried and ground to obtain the modified sepiolite-3.
[0035] Modified Sepiolite-4
[0036] The preparation process is similar to that of modified sepiolite-1, except that the volume of 2,4-cyclopentadiene-1-acetic acid used is 18 ml.
[0037] Modified Sepiolite-5
[0038] The preparation process is similar to that of modified sepiolite-3, except that the volume of cis-3-hexenoic acid used is 20 ml.
[0039] Modified Sepiolite-6
[0040] The preparation process is similar to that of modified sepiolite-3, except that in S3 only 2,4-cyclopentadiene-2-carboxylic acid is used to modify the acid-treated nano sepiolite.
[0041] Modified Sepiolite-7
[0042] The preparation process is similar to that of modified sepiolite-3, except that in S3 only cis-3-hexene is used to modify the acid-treated nano sepiolite.
[0043] The specific manufacturers and grades of the high-density polyethylene used in the following examples are Yanshan Petrochemical 3000JE, Shanghai Petrochemical YGH041, Dushanzi Petrochemical DMDA-8008H, and Maoming Petrochemical P4406C; the specific manufacturers and grades of the linear low-density polyethylene used are Yuanfeng Plastic AT6101, Qiaowei Chemical LL0220KJ, ExxonMobil 1002XBU, and Yangzi Petrochemical YLF-1801, which are not particularly limited herein.
[0044] Example 1
[0045] SS1: 20 parts of Yanshan Petrochemical 3000JE, 20 parts of Yuanfeng Plasticizing AT6101, 5 parts of modified sepiolite-1, 0.1 parts of triallyl cyanurate and 0.5 parts of dibutyl phthalate, 2 parts of antioxidant AO-30 and 1 part of oleamide were mixed and put into an internal mixer for melt blending at a mixing temperature of 120°C and a mixing time of 10 min to obtain a mixture;
[0046] SS2: The mixed material is added into a twin-screw extruder and extruded through four working zones to obtain pellets; wherein the working temperature of the first zone is 80°C, the working temperature of the second zone is 100°C, the working temperature of the third zone is 120°C, and the working temperature of the fourth zone is 120°C;
[0047] SS3: 0.5 parts of ethylene peroxide is heated and melted into a liquid for measurement, and mixed with the pellets obtained in SS2 at 80°C to allow the ethylene peroxide to diffuse into the interior of the pellets. The pellets are then added to a single-screw extruder and extruded into wires through two zones, wherein the operating temperature of the first zone is 80°C and the operating temperature of the second zone is 100°C; peroxide cross-linked polyethylene insulation material is obtained.
[0048] Example 2
[0049] SS1: 25 parts of Shanghai Petrochemical YGH041, 25 parts of Qiaowei Chemical LL0220KJ, 3 parts of modified sepiolite-2, 0.5 parts of triallyl isocyanurate, 1.2 parts of dioctyl phthalate, 5 parts of antioxidant 1010 and 2 parts of erucamide were mixed and put into an internal mixer for melt blending at a mixing temperature of 125°C and a mixing time of 9 minutes to obtain a mixture;
[0050] SS2: The mixed material is added into a twin-screw extruder and extruded into particles through four working zones to obtain pellets; wherein the working temperature of the first zone is 85°C, the working temperature of the second zone is 110°C, the working temperature of the third zone is 125°C, and the working temperature of the fourth zone is 125°C;
[0051] SS3: Heat and melt 1 part of monomethyl peroxide into liquid and measure it, mix it with the pellets obtained in SS2 at 90°C to allow the monomethyl peroxide to diffuse into the interior of the pellets, and then add it to a single-screw extruder and extrude it into wire through two zones, wherein the working temperature of the first zone is 85°C and the working temperature of the second zone is 110°C; obtain peroxide cross-linked polyethylene insulation material.
[0052] Example 3
[0053] SS1: 30 parts of DMDA-8008H from Dushanzi Petrochemical, 30 parts of LL0220KJ from Qiaowei Chemical, 1 part of modified sepiolite-3, 1.0 part of triallyl isocyanurate, 1.2 parts of dioctyl phthalate, 5 parts of antioxidant 168 and 5 parts of stearamide were mixed and put into an internal mixer for melt blending at a mixing temperature of 130°C and a mixing time of 8 min to obtain a mixture;
[0054] SS2: The mixed material is added into a twin-screw extruder and extruded into particles through four working zones to obtain pellets; wherein the working temperature of the first zone is 90°C, the working temperature of the second zone is 120°C, the working temperature of the third zone is 130°C, and the working temperature of the fourth zone is 130°C;
[0055] SS3: 2.1 parts of dicumyl peroxide were heated and melted into liquid for measurement, and mixed with the pellets obtained in SS2 at 100°C to diffuse the dicumyl peroxide into the interior of the pellets. The pellets were then added to a single-screw extruder and extruded into wires through two zones, wherein the operating temperature of the first zone was 90°C and the operating temperature of the second zone was 120°C; peroxide cross-linked polyethylene insulation material was obtained.
[0056] Example 4
[0057] The process is similar to that of Example 3, except that modified sepiolite-4 is used to replace modified sepiolite-3.
[0058] Example 5
[0059] The process is similar to that of Example 3, except that modified sepiolite-5 is used to replace modified sepiolite-3.
[0060] Comparative Example 1
[0061] The process is similar to that of Example 3, except that modified sepiolite-6 is used to replace modified sepiolite-3.
[0062] Comparative Example 2
[0063] The process is similar to that of Example 3, except that modified sepiolite-7 is used to replace modified sepiolite-3.
[0064] Comparative Example 3
[0065] The process is similar to that of Example 3, except that unmodified acid-treated nano-sepiolite is used instead of modified sepiolite-3.
[0066] Comparative Example 4
[0067] The process is similar to that of Example 3, except that 2,4-cyclopentadiene-1-carboxylic acid and cis-3-hexenoic acid converted in equal proportions are used to replace the modified sepiolite-3.
[0068] Performance Testing
[0069] Mechanical properties: GB / T1040.3-2006, requiring tensile strength ≥8.5MPa, elongation at break ≥250%;
[0070] Aging resistance: GB / T2951.12-2008 requires that under air heat aging (170℃ 240h), the tensile strength shall be ≥6.0MPa and the elongation at break shall be ≥100%; long-term aging resistance requires that under air heat aging (150℃, 1500h), there shall be no visual cracks after winding.
[0071] The specific test results are shown in Table 1:
[0072]
[0073] As can be seen from the data in Table 1, the performance of the peroxide cross-linked polyethylene insulating material prepared according to the technical solution provided by the present invention in Examples 1-5 meets the requirements. However, after receiving the air heat aging treatment, the insulating material of Examples 4-5 has a higher degree of mechanical property degradation than the insulating material of Examples 1-3. This is because the volume ratio of cyclopentadienoic acid to hexenoic acid in the modified sepiolite used is not in the preferred range. It can be seen that when preparing the modified sepiolite, the volume ratio of cyclopentadienoic acid to hexenoic acid used is in the preferred range, and the heat aging resistance of the obtained insulating material is more excellent. The results of Comparative Examples 1-2 illustrate that only one of cyclopentadienoic acid or hexenoic acid is used to modify sepiolite, and the long-term aging resistance of the cross-linked polyethylene insulating material prepared is unqualified, and the mechanical properties also significantly decrease. The results of Comparative Examples 3-4 illustrate that sepiolite, cyclopentadienoic acid and hexenoic acid have a synergistic effect on improving the heat aging resistance of peroxide cross-linked polyethylene insulating material.
[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A peroxide cross-linked polyethylene insulating material, characterized in that: The invention comprises the following raw materials by weight: 20-35 parts of high-density polyethylene, 20-30 parts of linear low-density polyethylene, 1-5 parts of modified sepiolite, 0.5-2.1 parts of peroxide cross-linking agent, 0.1-1 parts of auxiliary cross-linking agent and 0.5-15 parts of functional additive; wherein cyclopentadienoic acid and hexenoic acid are grafted on the surface of the modified sepiolite; and the cyclopentadienoic acid is at least one of 2,4-cyclopentadiene-1-acetic acid and 2,4-cyclopentadiene-1-carboxylic acid.
2. The peroxide cross-linked polyethylene insulation material according to claim 1, characterized in that: The preparation method of the modified sepiolite comprises the following steps: S1: Mix the nano-sepiolite and the acid solution in a solid-liquid ratio of 1-3 g: 10-16 ml, stir to fully react, centrifuge, filter, and wash until the pH of the final filtrate is neutral, and dry the obtained acid-treated nano-sepiolite for standby use; S2: Mix cyclopentadienoic acid, hexenoic acid and the acid-treated nano-sepiolite obtained in S1, drop concentrated sulfuric acid therein, heat under reflux to start the reaction, wait for the reaction to be completed, cool to room temperature, filter, dry and grind to obtain the modified sepiolite.
3. The peroxide cross-linked polyethylene insulating material according to claim 2, characterized in that: The concentration of the acid solution in S1 is 1-2 mol / L, and the type is at least one of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid.
4. The peroxide cross-linked polyethylene insulation material according to claim 2, characterized in that: The liquid-to-solid ratio of the cyclopentadienoic acid, hexenoic acid in S2 to the acid-treated nano-sepiolite obtained in S1 is 10-17 ml: 5-8 ml: 2-5 g.
5. The peroxide cross-linked polyethylene insulation material according to claim 1, characterized in that: The peroxide cross-linking agent is at least one of ethylene peroxide, monomethyl peroxide, and dicumyl peroxide.
6. The peroxide cross-linked polyethylene insulation material according to claim 1, characterized in that: The auxiliary cross-linking agent is at least one of triallyl cyanurate, triallyl isocyanurate, and propane trimethanol triacrylate.
7. The peroxide cross-linked polyethylene insulation material according to claim 1, characterized in that: The functional additive is at least one of a plasticizer, an antioxidant and a lubricant.
8. The peroxide cross-linked polyethylene insulation material according to claim 7, characterized in that: The antioxidant is at least one of hydroxylated antioxidants, alkyl biphenyl antioxidants, and hydroxyphosphonate antioxidants; the lubricant is at least one of oleamide, erucamide, stearamide, and ethylene bisstearamide.
9. The method for preparing the peroxide cross-linked polyethylene insulation material according to any one of claims 1 to 8, characterized in that: The following steps are involved: SS1: Mix all raw material components except the peroxide crosslinking agent according to the formula and put them into an internal mixer for melt blending at a mixing temperature of 120-150°C for 8-10 minutes to obtain a mixed material; SS2: Add the mixed material into a twin-screw extruder and extrude it through four working zones to obtain pellets; wherein the working temperature of the first zone is 80-90°C, the working temperature of the second zone is 100-110°C, the working temperature of the third zone is 120-130°C, and the working temperature of the fourth zone is 120-130°C; SS3: The peroxide cross-linking agent is heated and melted into a liquid for metering, and mixed with the pellets obtained in SS2 at 80-100°C to diffuse the peroxide cross-linking agent into the interior of the pellets, and then added to a single-screw extruder and extruded into wires through two zones, wherein the working temperature of the first zone is 80-90°C and the working temperature of the second zone is 100-120°C; peroxide cross-linked polyethylene insulation material is obtained.
Citation Information
Patent Citations
Flexible cross-linked polyethylene insulated cable material and preparation method of cable material
CN103865156A
Preparation method of high-voltage direct-current polyethylene cable insulation material
CN110669276A
Thermoplastic crosslinked polyethylene material, preparation method and use thereof
US20200087491A1