A packaging film and its preparation method and application

By using a packaging film composed of an adhesive layer, an ion exchange layer and a corrosion-resistant layer in a double-glass package LECO component, the problem of insufficient performance of the EVA packaging film is solved, and the compatibility and corrosion resistance of solar cell modules are improved. , reduces power attenuation.

CN118599438BActive Publication Date: 2024-11-05ZHEJIANG SOLARTRON TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411074129.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing EVA packaging films exhibit insufficient volume resistivity, water vapor transmittance and corrosion resistance in double-glass packaging LECO components, resulting in poor packaging effect and affecting the power attenuation of solar cell modules.

Method used

The encapsulation film consisting of an adhesive layer, an ion exchange layer and an anti-corrosion layer is adopted. The adhesive layer uses EVA resin, the ion exchange layer contains cation exchange resin, and the corrosion resistance layer uses EVA resin and acid remover, and passes a crosslinking agent. and light stabilizers improve compatibility and crosslinking density.

Benefits of technology

Improves the compatibility and crosslinking density of the packaging film, reduces the risk of delamination after component aging, blocks the migration of sodium ions, improves PID phenomenon, extends the adhesion and corrosion resistance of the component, and reduces power. attenuation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118599438B_ABST
    Figure CN118599438B_ABST
Patent Text Reader

Abstract

The invention discloses a packaging film and a preparation method and application thereof, belonging to the technical field of solar cell modules. The packaging film comprises an adhesive layer, an ion exchange layer and an anti-corrosion layer arranged in sequence; the first matrix resin of the adhesive layer is a first EVA resin; the second matrix resin of the ion exchange layer comprises a cation exchange resin; wherein the cation exchange resin comprises an acrylic resin; and the third matrix resin of the anti-corrosion layer is a third EVA resin. The various layers of the packaging film have good compatibility, the acrylic resin in the ion exchange layer can adsorb sodium ions migrating from the glass side during the aging process, and prevent the sodium ions from corroding the battery sheet. The packaging film has good bonding force and anti-corrosion ability, can reduce the power attenuation of solar cells, and broaden the application scope of the EVA packaging film in the market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell modules, and in particular to a packaging adhesive film and a preparation method and application thereof. Background Art

[0002] The laser-assisted sintering technology (LECO) currently used in N-type TOPCon cells has attracted much attention. In addition, the silver-aluminum dual plasma of TOPCon cells has been replaced with pure silver plasma, which alleviates the disadvantage of N-type TOPCon cells being sensitive to water vapor and prone to corrosion.

[0003] Common double-glass encapsulated LECO modules adopt a double-glass encapsulation solution that uses EPE (polyethylene foam board) encapsulation film and EVA (ethylene-vinyl acetate copolymer) encapsulation film, or EPE encapsulation film and EPE encapsulation film. However, the performance of EVA encapsulation film is difficult to meet the needs of double-glass encapsulated LECO modules. For example, the volume resistivity, water vapor permeability and corrosion resistance of EVA are much lower than those of POE resin (polyolefin elastomer) in the encapsulation film, resulting in poor encapsulation effect, affecting the power attenuation and other performance of solar cell modules.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a packaging adhesive film and a preparation method and application thereof, so as to solve or improve the above technical problems.

[0006] The present invention can be implemented like this:

[0007] In a first aspect, the present invention provides a packaging film, which includes an adhesive layer, an ion exchange layer and an anti-corrosion layer arranged in sequence;

[0008] The first matrix resin of the bonding layer is a first EVA resin;

[0009] The second matrix resin of the ion exchange layer includes a cation exchange resin; wherein the cation exchange resin includes an acrylic resin;

[0010] The third base resin of the anti-corrosion layer is a third EVA resin.

[0011] In an optional embodiment, the second base resin further includes a second EVA resin, and the weight ratio of the second EVA resin to the cation exchange resin is 9:1 to 7:3.

[0012] In an optional embodiment, the cation exchange resin further includes at least one of a sulfonic acid cation exchange resin, a phosphoric acid cation exchange resin, a phenolic cation exchange resin and other carboxylic acid cation exchange resins.

[0013] In an optional embodiment, the raw materials for preparing the bonding layer also include a first co-crosslinking agent, the raw materials for preparing the ion exchange layer also include a second co-crosslinking agent, and the raw materials for preparing the anti-corrosion layer also include a third co-crosslinking agent; the first co-crosslinking agent, the second co-crosslinking agent, and the third co-crosslinking agent independently include at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane triethoxy acrylate, triallyl isocyanate, ethoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate, tetrafunctional polyester acrylate, and 1,6-hexanediol diacrylate.

[0014] In an optional embodiment, the raw materials for preparing the bonding layer further include coupling agent oligomers; the coupling agent oligomers include at least one of vinyl coupling agent oligomers, bisamino coupling agent oligomers, epoxy coupling agent oligomers, alkoxy coupling agent oligomers and methacryloxy coupling agent oligomers.

[0015] In an optional embodiment, the raw materials for preparing the anti-corrosion layer further include an acid scavenger; the acid scavenger includes at least one of magnesium oxide, magnesium hydroxide, magnesium silicate, hydrotalcite, silicon dioxide, calcium stearate, zinc oxide and zirconium phosphate.

[0016] In an optional embodiment, the raw materials for preparing the bonding layer include, by weight: 100 parts of a first base resin, 0.1 to 2 parts of a first peroxide cross-linking agent, 0.1 to 2 parts of a first auxiliary cross-linking agent, 0.1 to 2 parts of a first coupling agent, 0.1 to 2 parts of a coupling agent oligomer, and 0.01 to 1 parts of a first light stabilizer.

[0017] In an optional embodiment, the raw materials for preparing the bonding layer include, by weight: 100 parts of a first base resin, 0.4 to 1.2 parts of a first peroxide cross-linking agent, 0.4 to 1.2 parts of a first auxiliary cross-linking agent, 0.2 to 0.8 parts of a first coupling agent, 0.1 to 0.4 parts of a coupling agent oligomer, and 0.05 to 0.4 parts of a first light stabilizer.

[0018] In an optional embodiment, the raw materials for preparing the ion exchange layer include, by weight: 20 to 100 parts of a second base resin, 0.1 to 2 parts of a second peroxide cross-linking agent, 0.1 to 2 parts of a second auxiliary cross-linking agent, 0.1 to 2 parts of a second coupling agent, and 0.01 to 1 parts of a second light stabilizer.

[0019] In an optional embodiment, the raw materials for preparing the ion exchange layer include, by weight: 100 parts of a second base resin, 0.4 to 1.2 parts of a second peroxide cross-linking agent, 0.4 to 1.2 parts of a second auxiliary cross-linking agent, 0.2 to 0.8 parts of a second coupling agent, and 0.05 to 0.4 parts of a second light stabilizer.

[0020] In an optional embodiment, the second base resin includes 0 to 100 parts of a second EVA resin, more than 0 and no more than 100 parts of a cation exchange resin, and 0.1 to 2 parts of a third coupling agent, by weight.

[0021] In an optional embodiment, the second base resin includes 50 to 80 parts of a second EVA resin, 20 to 50 parts of a cation exchange resin, and 0.1 to 2.0 parts of a third coupling agent, by weight.

[0022] In an optional embodiment, the raw materials for preparing the anti-corrosion layer include, by weight: 100 parts of a third base resin, 0.1 to 2 parts of a third peroxide cross-linking agent, 0.1 to 2 parts of a third auxiliary cross-linking agent, 0.1 to 2 parts of a fourth coupling agent, 0.01 to 1 parts of an acid scavenger, and 0.01 to 1 parts of a third light stabilizer.

[0023] In an optional embodiment, the raw materials for preparing the anti-corrosion layer include, by weight: 100 parts of a third base resin, 0.4 to 1.2 parts of a third peroxide cross-linking agent, 0.4 to 1.2 parts of a third auxiliary cross-linking agent, 0.2 to 0.8 parts of a fourth coupling agent, 0.05 to 0.4 parts of an acid scavenger, and 0.05 to 0.4 parts of a third light stabilizer.

[0024] In an optional embodiment, the first peroxide crosslinking agent, the second peroxide crosslinking agent and the third peroxide crosslinking agent independently include at least one of tert-butyl peroxycarbonate-2-ethylhexyl ester, tert-amyl peroxy(2-ethylhexyl)carbonate, tert-butyl peroxybenzoate, tert-butyl peroxyacetate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate and diisopropylbenzene peroxide.

[0025] In an optional embodiment, the first coupling agent, the second coupling agent, the third coupling agent, the fourth coupling agent and the fourth coupling agent independently include at least one of vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane and vinyltri-tert-butoxysilane.

[0026] In an optional embodiment, the first light stabilizer, the second light stabilizer and the third light stabilizer are independently hindered amine light stabilizers.

[0027] In an optional embodiment, the first light stabilizer, the second light stabilizer and the third light stabilizer independently include at least one of bis-2,2,6,6-tetramethylpiperidinol sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate and bis(2,2,6,6-tetramethyl-4-piperidinol) sebacate.

[0028] In an optional embodiment, the thickness of the bonding layer is 0.10 mm to 0.60 mm; or the thickness of the ion exchange layer is 0.10 mm to 0.60 mm; or the thickness of the anti-corrosion layer is 0.10 mm to 0.60 mm.

[0029] In an optional embodiment, the thickness of the packaging film is 0.3 mm to 0.9 mm.

[0030] In a second aspect, the present invention provides a method for preparing an encapsulation adhesive film as described in any of the aforementioned embodiments, comprising the following steps: extruding, casting and calendering a first masterbatch prepared from the raw materials for preparing a bonding layer, a second masterbatch prepared from the raw materials for preparing an ion exchange layer, and a third masterbatch prepared from the raw materials for preparing an anti-corrosion layer.

[0031] In an optional embodiment, the preparation of the first masterbatch includes: mixing the raw materials for preparing the bonding layer at a temperature of 40° C. to 50° C.

[0032] In an optional embodiment, the preparation of the second masterbatch includes: melt-blending the second EVA resin, the cation exchange resin and the third coupling agent at 80°C~150°C and granulating to obtain a base masterbatch, and then mixing the base masterbatch with the second peroxide cross-linking agent, the second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer at 40°C~50°C.

[0033] In an optional embodiment, the preparation of the third masterbatch includes: mixing the raw materials for preparing the anti-corrosion layer at a temperature of 40° C. to 50° C.

[0034] In an optional embodiment, the temperature of the tape casting process is 70°C to 110°C.

[0035] In a third aspect, the present invention provides a solar cell module, wherein the solar cell module comprises the encapsulation film of any one of the aforementioned embodiments.

[0036] In an optional embodiment, the solar cell assembly includes a first glass layer, a first encapsulation film layer, a battery cell, a second encapsulation film layer and a second glass layer arranged in sequence from bottom to top;

[0037] The encapsulation films in the first encapsulation film layer and the second encapsulation film layer are both the above-mentioned encapsulation films.

[0038] The beneficial effects of the present invention include:

[0039] The encapsulation film provided by the present invention has good compatibility of the base resins of each layer, so that the compatibility between the layers is good. On the one hand, it solves the incompatibility problem of EVA resin and POE resin in the existing encapsulation film due to the large structural difference; on the other hand, it solves the problem of EPE film additive migration caused by the different polarities of POE resin and additives, thereby reducing the risk of delamination after component aging.

[0040] The middle layer contains cation exchange resin, which can hydrolyze hydrogen ions during the aging process of the component. The remaining negatively charged groups after hydrolysis can adsorb and combine with sodium ions, effectively blocking the migration of sodium ions, thereby improving or solving the PID phenomenon of double-glass components.

[0041] Therefore, the encapsulation film provided by the present invention can provide long-lasting and effective adhesion and corrosion resistance for component encapsulation, reduce the power attenuation of the component, and broaden the application scope of the EVA encapsulation film in the double-glass component market. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0043] Figure 1 A schematic diagram of the structure of the encapsulation film provided by the present invention;

[0044] Figure 2 It is a schematic diagram of the structure of the double-glass component in the present invention.

[0045] Icons: 10-encapsulation film; 11-adhesive layer; 12-ion exchange layer; 13-anti-corrosion layer; 21-first glass layer; 22-first encapsulation film layer; 23-battery cell; 24-second encapsulation film layer; 25-second glass layer. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0047] The encapsulation adhesive film provided by the present invention and its preparation method and application are described in detail below.

[0048] like Figure 1 As shown, the present invention provides a packaging film 10, which includes an adhesive layer 11, an ion exchange layer 12 and an anti-corrosion layer 13 arranged in sequence. The packaging film 10 can be used in a solar cell module (such as a double-glass module).

[0049] Each layer of the three-layer packaging film 10 has a different function. For example, the packaging film 10 used in a double-glass component (such as Figure 2 As shown in the figure, the adhesive layer 11 in the packaging film 10 is used to adhere to the glass. The adhesive layer can provide long-lasting and effective bonding force for the component packaging to prevent delamination and the generation of bubbles; the anti-corrosion layer 13 is used to adhere to the battery cell 23 to prevent the battery surface from being corroded by water vapor and acid; the ion exchange layer 12 serves as an intermediate layer to absorb the sodium ions released from the glass side to avoid the generation of component PID (potential induced decay) phenomenon.

[0050] The raw material for preparing the above-mentioned bonding layer 11 includes a first base resin, and the first base resin is a first EVA resin.

[0051] The raw material for preparing the ion exchange layer 12 includes a second matrix resin, which includes a cation exchange resin; wherein the cation exchange resin includes an acrylic resin; on this basis, the cation exchange resin can further include at least one of a sulfonic acid cation exchange resin, a phosphoric acid cation exchange resin, a phenolic cation exchange resin and other carboxylic acid cation exchange resins.

[0052] In some embodiments, the second matrix resin includes 0 to 100 parts of the second EVA resin and greater than 0 and no more than 100 parts of the cation exchange resin by weight. In some typical embodiments, the second matrix resin includes both the second EVA resin and the cation exchange resin. For example, the weight ratio of the second EVA resin to the cation exchange resin can be 9:1 to 7:3, such as 9:1, 8.5:1.5, 8:2, 7.5:2.5 or 7:3.

[0053] The raw material for preparing the anti-corrosion layer 13 includes a third matrix resin, and the third matrix resin is a third EVA resin.

[0054] The base resins of each layer of the above-mentioned packaging film 10 have good compatibility, which makes the compatibility between the layers good. On the one hand, it solves the incompatibility problem between the EVA resin and the POE resin in the existing packaging film 10 due to the large structural difference; on the other hand, it solves the problem of EPE film additive migration caused by the different polarities of POE resin and additives, thereby reducing the risk of delamination after component aging.

[0055] The middle layer contains cation exchange resin, which can hydrolyze hydrogen ions during the aging process of the component. The remaining negatively charged groups after hydrolysis can adsorb and combine with sodium ions, effectively blocking the migration of sodium ions, thereby improving or solving the PID phenomenon of double-glass components.

[0056] Therefore, the packaging film 10 provided by the present invention can provide long-lasting and effective bonding force and corrosion resistance for component packaging, reduce the power attenuation of the component, and broaden the application scope of the EVA packaging film 10 in the double-glass component market.

[0057] Furthermore, the raw materials for preparing the above-mentioned bonding layer 11 also include a first auxiliary cross-linking agent, the raw materials for preparing the ion exchange layer 12 also include a second auxiliary cross-linking agent, and the raw materials for preparing the anti-corrosion layer 13 also include a third auxiliary cross-linking agent.

[0058] The first co-crosslinking agent, the second co-crosslinking agent, and the third co-crosslinking agent independently include at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane triethoxyacrylate, triallyl isocyanate, ethoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate, tetrafunctional polyester acrylate, and 1,6-hexanediol diacrylate. Using a co-crosslinking agent in each layer, especially using an acrylate oligomer with multiple functional groups as a co-crosslinking agent, can enhance the crosslinking speed and crosslinking density of the EVA film, and improve the volume resistivity and water barrier of the film. In particular, tetrafunctional polyester acrylate is used as a co-crosslinking agent. The tetrafunctional polyester acrylate contains abundant C=C double bonds in its molecular structure, which can provide a large number of reactive active sites in the crosslinking process of EVA segments, and can accelerate the crosslinking speed and increase the crosslinking density compared with ordinary small molecule crosslinking agents. Moreover, based on the structural characteristics of the tetrafunctional polyester acrylate oligomer, the network structure of the EVA film after crosslinking can be made denser.

[0059] Furthermore, the raw materials for preparing the above-mentioned adhesive layer 11 also include coupling agent oligomers. The coupling agent oligomers include at least one of vinyl coupling agent oligomers, bisamino coupling agent oligomers, epoxy coupling agent oligomers, alkoxy coupling agent oligomers and methacryloxy coupling agent oligomers.

[0060] Furthermore, the raw materials for preparing the above-mentioned anti-corrosion layer 13 also include an acid scavenger; the acid scavenger includes at least one of magnesium oxide, magnesium hydroxide, magnesium silicate, hydrotalcite, silicon dioxide, calcium stearate, zinc oxide and zirconium phosphate.

[0061] The anti-corrosion layer 13 uses an acid scavenger to neutralize the weak acid in the EVA film and effectively block the water vapor and acid of the battery.

[0062] In parts by weight, the raw materials for preparing the bonding layer 11 may include: 100 parts of a first EVA resin, 0.1 to 2 parts of a first peroxide cross-linking agent, 0.1 to 2 parts of a first auxiliary cross-linking agent, 0.1 to 2 parts of a first coupling agent, 0.1 to 2 parts of a coupling agent oligomer, and 0.01 to 1 parts of a first light stabilizer.

[0063] Among them, the amounts of the first peroxide crosslinking agent, the first auxiliary crosslinking agent, the first coupling agent and the coupling agent oligomer in the bonding layer 11 can independently be 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts or 2 parts, etc., and can also independently be other values ​​within the range of 0.1 to 2 parts.

[0064] The amount of the first light stabilizer in the adhesive layer 11 may be 0.01 part, 0.05 part, 0.1 part, 0.2 part, 0.5 part, 0.8 part or 1 part, etc., or may be other values ​​within the range of 0.01 to 1 part.

[0065] In some preferred embodiments, the raw materials for preparing the bonding layer 11 may include: 100 parts of a first EVA resin, 0.4 to 1.2 parts (such as 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts or 1.2 parts, etc.) of a first peroxide cross-linking agent, 0.4 to 1.2 parts (such as 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts or 1.2 parts, etc.) of a first auxiliary cross-linking agent, 0.2 to 0.8 parts (such as 0.2 parts, 0.4 parts, 0.6 parts or 0.8 parts, etc.) of a first coupling agent, 0.1 to 0.4 parts (such as 0.1 parts, 0.2 parts, 0.3 parts or 0.4 parts, etc.) of a coupling agent oligomer, and 0.05 to 0.4 parts (such as 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts or 0.4 parts, etc.) of a first light stabilizer.

[0066] In some preferred embodiments, the raw materials for preparing the bonding layer 11 may include: 100 parts of a first EVA resin, 0.8 parts of a first peroxide cross-linking agent, 0.6 parts of a first auxiliary cross-linking agent, 0.4 parts of a first coupling agent, 0.1 parts of a coupling agent oligomer, and 0.2 parts of a first light stabilizer.

[0067] By weight, the raw materials for preparing the ion exchange layer 12 may include: 20-100 parts of a second base resin, 0.1-2 parts of a second peroxide crosslinking agent, 0.1-2 parts of a second auxiliary crosslinking agent, 0.1-2 parts of a second coupling agent, and 0.01-1 parts of a second light stabilizer.

[0068] The amount of the second matrix resin in the ion exchange layer 12 may be 20 parts, 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts or 100 parts, or other values ​​within the range of 20 to 100 parts.

[0069] The amounts of the second peroxide crosslinking agent, the second auxiliary crosslinking agent and the second coupling agent in the ion exchange layer 12 can independently be 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts or 2 parts, etc., and can also independently be other values ​​within the range of 0.1 to 2 parts.

[0070] The amount of the second light stabilizer in the ion exchange layer 12 can be 0.01 part, 0.05 part, 0.1 part, 0.2 part, 0.5 part, 0.8 part or 1 part, etc., and can also be other values ​​within the range of 0.01 to 1 part.

[0071] In some preferred embodiments, the raw materials for preparing the ion exchange layer 12 may include: 100 parts of a second base resin, 0.4 to 1.2 parts (such as 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts or 1.2 parts, etc.) of a second peroxide cross-linking agent, 0.4 to 1.2 parts (such as 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts or 1.2 parts, etc.) of a second auxiliary cross-linking agent, 0.2 to 0.8 parts (such as 0.2 parts, 0.4 parts, 0.6 parts or 0.8 parts, etc.) of a second coupling agent, and 0.05 to 0.4 parts (such as 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts or 0.4 parts, etc.) of a second light stabilizer.

[0072] In some preferred embodiments, the raw materials for preparing the ion exchange layer 12 may include: 100 parts of a second base resin, 0.8-1.0 parts of a second peroxide crosslinking agent, 0.5-0.7 parts of a second auxiliary crosslinking agent, 0.4-0.5 parts of a second coupling agent, and 0.2 parts of a second light stabilizer.

[0073] In parts by weight, the raw materials for preparing the second base resin may include 0 to 100 parts of a second EVA resin, more than 0 and no more than 100 parts of a cation exchange resin, and 0.1 to 2 parts of a third coupling agent.

[0074] The amount of the second EVA resin in the second matrix resin can be 0 parts, 5 parts, 10 parts, 20 parts, 40 parts, 60 parts, 80 parts or 100 parts, etc., or other values ​​within the range of 0 to 100 parts.

[0075] The amount of the cation exchange resin in the second matrix resin can be 0.01 parts, 0.1 parts, 1 parts, 5 parts, 10 parts, 20 parts, 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts or 100 parts, etc., or it can be other values ​​within the range of greater than 0 and not exceeding 100 parts.

[0076] The third coupling agent can be used in an amount of 0.1, 0.2, 0.5, 0.8, 1, 1.2, 1.5, 1.8 or 2 parts in the second matrix resin, and can also be independently used in an amount of other values ​​within the range of 0.1 to 2 parts.

[0077] In some preferred embodiments, the second base resin includes 50-80 parts (such as 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts or 80 parts, etc.) of a second EVA resin, 20-50 parts (such as 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts or 50 parts, etc.) of a cation exchange resin and 0.1-2.0 parts (such as 0.1 parts, 0.5 parts, 1.0 parts, 1.5 parts or 2.0 parts, etc.) of a third coupling agent.

[0078] In some preferred embodiments, the second base resin includes 80 parts of a second EVA resin, 20 parts of a cation exchange resin, and 0.4-1.0 parts of a third coupling agent.

[0079] In parts by weight, the raw materials for preparing the anti-corrosion layer 13 may include: 100 parts of a third EVA resin, 0.1 to 2 parts of a third peroxide cross-linking agent, 0.1 to 2 parts of a third auxiliary cross-linking agent, 0.1 to 2 parts of a fourth coupling agent, 0.01 to 1 parts of an acid scavenger, and 0.01 to 1 parts of a third light stabilizer.

[0080] Among them, the amounts of the third peroxide crosslinking agent, the third auxiliary crosslinking agent and the fourth coupling agent in the anti-corrosion layer 13 can independently be 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts or 2 parts, etc., and can also independently be other values ​​within the range of 0.1 to 2 parts.

[0081] The amounts of the acid scavenger and the third light stabilizer used in the anti-corrosion layer 13 can be independently 0.01 parts, 0.05 parts, 0.1 parts, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts or 1 parts, etc., or other values ​​within the range of 0.01 to 1 parts.

[0082] In some preferred embodiments, the raw materials for preparing the anti-corrosion layer 13 may include: 100 parts of a third base resin, 0.4 to 1.2 parts (such as 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts or 1.2 parts, etc.) of a third peroxide cross-linking agent, 0.4 to 1.2 parts (such as 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts or 1.2 parts, etc.) of a third auxiliary cross-linking agent, 0.2 to 0.8 parts (such as 0.2 parts, 0.4 parts, 0.6 parts or 0.8 parts, etc.) of a fourth coupling agent, 0.05 to 0.4 parts (such as 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts or 0.4 parts, etc.) of an acid scavenger, and 0.05 to 0.4 parts (such as 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts or 0.4 parts, etc.) of a third light stabilizer.

[0083] In some preferred embodiments, the raw materials for preparing the anti-corrosion layer 13 may include: 100 parts of a third base resin, 1.0-1.2 parts of a third peroxide cross-linking agent, 0.6-0.9 parts of a third auxiliary cross-linking agent, 0.4 parts of a fourth coupling agent, 0.2 parts of an acid scavenger, and 0.1 parts of a third light stabilizer.

[0084] In some optional embodiments, the first peroxide crosslinking agent, the second peroxide crosslinking agent and the third peroxide crosslinking agent can independently include at least one of tert-butyl peroxycarbonate-2-ethylhexyl ester, tert-amyl peroxy (2-ethylhexyl) carbonate, tert-butyl peroxybenzoate, tert-butyl peroxyacetate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate and diisopropylbenzene peroxide.

[0085] In some optional embodiments, the first coupling agent, the second coupling agent, the third coupling agent, the fourth coupling agent and the fourth coupling agent can independently include at least one of vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane and vinyltri-tert-butoxysilane.

[0086] In some optional embodiments, the first light stabilizer, the second light stabilizer and the third light stabilizer can all be independently hindered amine light stabilizers. In some preferred embodiments, the first light stabilizer, the second light stabilizer and the third light stabilizer can all independently include at least one of bis-2,2,6,6-tetramethylpiperidinol sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate and bis(2,2,6,6-tetramethyl-4-piperidinol) sebacate.

[0087] As mentioned above, with respect to the encapsulation film 10 provided by the present invention, the base material of each layer thereof preferably contains EVA resin, and the compatibility between the layers is good. On the one hand, the incompatibility problem due to the large structural difference between the EVA resin and the POE resin in the existing encapsulation film 10 is solved; on the other hand, the problem of EPE film additive migration caused by the different polarities of the POE resin and the additive is solved, thereby reducing the risk of delamination after component aging.

[0088] The middle layer preferably uses acrylic resin as the cation exchange resin, which has weak polarity and good compatibility with EVA resin. In addition, acrylic resin can hydrolyze hydrogen ions during the aging process of the component. The negatively charged groups remaining after the hydrolysis of the acrylic resin can be adsorbed and combined with sodium ions, effectively blocking the migration of sodium ions, thereby improving or solving the PID phenomenon of the double-glass component.

[0089] In addition, the use of co-crosslinking agents in each layer, especially the use of multifunctional acrylate oligomers as co-crosslinking agents, can enhance the crosslinking speed and crosslinking density of the EVA film, and improve the volume resistivity and water barrier properties of the film. In particular, the use of tetrafunctional polyester acrylate as a co-crosslinking agent, which contains abundant C=C double bonds in its molecular structure, can provide a large number of reactive sites in the crosslinking process of the EVA chain segments, and can accelerate the crosslinking speed and increase the crosslinking density compared to ordinary small molecule crosslinking agents; and, based on the structural characteristics of tetrafunctional polyester acrylate oligomers, it can make the network structure of the EVA film after crosslinking more dense.

[0090] In addition, the anti-corrosion layer 13 uses an acid scavenger to neutralize the weak acid in the EVA film and effectively block the water vapor and acid of the battery.

[0091] Therefore, the packaging film 10 provided by the present invention can provide long-lasting and effective bonding force and corrosion resistance for component packaging, reduce the power attenuation of the component, and broaden the application scope of the EVA packaging film 10 in the double-glass component market.

[0092] In some embodiments, the thickness of the adhesive layer 11, the ion exchange layer 12 and the anti-corrosion layer 13 can be independently 0.10 mm to 0.60 mm, such as 0.10 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm or 0.6 mm, etc., or other values ​​within the range of 0.10 mm to 0.60 mm. In some typical embodiments, the total thickness of the packaging film 10 can be 0.3 mm to 0.9 mm, such as 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm or 0.9 mm, etc.

[0093] Correspondingly, the present invention also provides a method for preparing the above-mentioned encapsulation film 10, comprising the following steps: extruding, casting and calendering a first masterbatch prepared from the raw materials for preparing the bonding layer 11, a second masterbatch prepared from the raw materials for preparing the ion exchange layer 12, and a third masterbatch prepared from the raw materials for preparing the anti-corrosion layer 13.

[0094] In some enumerated methods, the first masterbatch, the second masterbatch and the third masterbatch can be respectively fed into a single screw extruder from three hoppers, and divided into upper, middle and lower layers by a distributor at the die head, and a transparent EVA encapsulation film 10 can be prepared by casting and calendering.

[0095] The temperature of the casting process can be 70°C to 110°C, such as 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C or 110°C, or any other value within the range of 70°C to 110°C.

[0096] In some embodiments, the preparation of the first masterbatch may include: mixing the raw materials for preparing the bonding layer 11 at 40°C to 50°C. The mixing temperature may be 40°C, 45°C, or 50°C, or other values ​​within the range of 40°C to 50°C.

[0097] Specifically, the first cross-linking agent, the first coupling agent, the coupling agent oligomer and the first light stabilizer may be pre-dissolved and mixed to obtain a first intermediate mixing aid; the first EVA resin and the first peroxide are fully stirred and then the first intermediate mixing aid is added, and the mixture is further stirred and mixed at a temperature of 40° C. to 50° C. to allow the first intermediate mixing aid to be fully absorbed.

[0098] In some embodiments, the preparation of the second masterbatch may include: melt blending the second EVA resin, the cation exchange resin and the third coupling agent at 80°C to 150°C and then granulating to obtain a matrix masterbatch, and then mixing the matrix masterbatch with the second peroxide crosslinking agent, the second auxiliary crosslinking agent, the second coupling agent and the second light stabilizer at 40°C to 50°C. The temperature of the melt mixing of the second EVA resin, the cation exchange resin and the third coupling agent may be 80°C to 150°C, such as 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, or any other value within the range of 80°C to 150°C. The mixing temperature of the matrix masterbatch with the second peroxide crosslinking agent, the second auxiliary crosslinking agent, the second coupling agent and the second light stabilizer may be 40°C, 45°C or 50°C, or any other value within the range of 40°C to 50°C.

[0099] Specifically, the second EVA resin, the cation exchange resin and the third coupling agent can be melt-mixed and extruded through a twin-screw granulator, and then cooled and pelletized to obtain a matrix masterbatch. The second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer are pre-dissolved and mixed to obtain a second intermediate mixing auxiliary agent; the matrix masterbatch and the second peroxide cross-linking agent are fully stirred and then added to the second intermediate mixing auxiliary agent, and further stirred and mixed at a temperature of 40°C to 50°C to allow the second intermediate mixing auxiliary agent to be fully absorbed.

[0100] In some embodiments, the preparation of the third masterbatch includes: mixing the raw materials for preparing the anti-corrosion layer 13 at 40°C to 50°C. The mixing temperature may be 40°C, 45°C, or 50°C, or other values ​​within the range of 40°C to 50°C.

[0101] Specifically, the third auxiliary cross-linking agent, the fourth coupling agent, the acid scavenger and the third light stabilizer may be pre-dissolved and mixed to obtain a third intermediate mixing auxiliary agent; the third EVA resin and the third peroxide are fully stirred and then the third intermediate mixing auxiliary agent is added, and the mixture is further stirred and mixed at a temperature of 40° C. to 50° C. to allow the third intermediate mixing auxiliary agent to be fully absorbed.

[0102] As mentioned above, the encapsulation film 10 provided by the present invention has a simple preparation process flow and takes into account both low cost and high reliability.

[0103] In addition, the present invention also provides a solar cell assembly, which comprises the above-mentioned packaging adhesive film 10 .

[0104] In some embodiments, the solar cell module may be a single-glass module or a double-glass module.

[0105] Take the solar cell module as a double glass module as an example. Figure 2 The solar cell assembly includes a first glass layer 21, a first encapsulation film layer 22, a battery cell 23, a second encapsulation film layer 24 and a second glass layer 25 arranged in sequence from bottom to top; wherein the encapsulation films 10 in the first encapsulation film layer 22 and the second encapsulation film layer 24 are both the above-mentioned encapsulation films 10 provided by the present invention.

[0106] The solar cell module having the encapsulation film 10 can obtain lower water vapor transmission rate, higher peel strength and lower power attenuation.

[0107] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0108] Example 1

[0109] This embodiment provides a packaging adhesive film 10, which includes an adhesive layer 11, an ion exchange layer 12 and an anti-corrosion layer 13 arranged in sequence.

[0110] The raw materials for preparing the bonding layer 11 include, by weight, 100 parts by weight of a first EVA resin, 0.8 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (a first peroxide crosslinking agent), 0.6 parts by weight of triallyl isocyanurate (a first auxiliary crosslinking agent), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a first coupling agent), 0.1 parts by weight of a vinyl silane oligomer (a coupling agent oligomer), and 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a first light stabilizer).

[0111] In terms of weight parts, the raw materials for preparing the ion exchange layer 12 include: 100 weight parts of the second base resin, 0.8 weight parts of tert-butyl peroxycarbonate-2-ethylhexyl ester (second peroxide crosslinking agent), 0.5 weight parts of triallyl isocyanurate (second auxiliary crosslinking agent), 0.4 weight parts of γ-methacryloxypropyl trimethoxysilane (second coupling agent), and 0.2 weight parts of bis-2,2,6,6-tetramethylpiperidinol sebacate (second light stabilizer). Among them, the second base resin includes 20 weight parts of acrylic resin (cation exchange resin), 80 weight parts of the second EVA resin, and 0.4 weight parts of γ-methacryloxypropyl trimethoxysilane (third coupling agent);

[0112] In parts by weight, the raw materials for preparing the anti-corrosion layer 13 include: 100 parts by weight of a third EVA resin, 1.0 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (a third peroxide crosslinking agent), 0.9 parts by weight of a third auxiliary crosslinking agent (0.6 parts by weight of triallyl isocyanurate and 0.3 parts by weight of a tetrafunctional polyester acrylate), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a fourth coupling agent), 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a third light stabilizer), and 0.1 parts of zirconium phosphate (acid scavenger).

[0113] The preparation method of the packaging film 10 includes:

[0114] S1: pre-dissolve and mix the first co-crosslinking agent, the first coupling agent, the coupling agent oligomer and the first light stabilizer to obtain a first intermediate mixing auxiliary agent; fully stir the first EVA resin and the first peroxide, then add the first intermediate mixing auxiliary agent, and further stir and mix at a temperature of 45° C. to fully absorb the first intermediate mixing auxiliary agent to obtain a first masterbatch;

[0115] S2: The second EVA resin, the cation exchange resin and the third coupling agent are melt-mixed and extruded through a twin-screw granulator, and then cooled and pelletized to obtain a matrix masterbatch. The second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer are pre-dissolved and mixed to obtain a second intermediate mixing auxiliary agent; the matrix masterbatch and the second peroxide cross-linking agent are fully stirred and then the second intermediate mixing auxiliary agent is added, and further stirred and mixed at a temperature of 45°C to allow the second intermediate mixing auxiliary agent to be fully absorbed to obtain a second masterbatch;

[0116] S3: Pre-dissolve and mix the third co-crosslinking agent, the fourth coupling agent, the acid scavenger and the third light stabilizer to obtain a third intermediate mixing auxiliary agent; fully stir the third EVA resin and the third peroxide, then add the third intermediate mixing auxiliary agent, further stir and mix at a temperature of 45°C to allow the third intermediate mixing auxiliary agent to be fully absorbed, and obtain a third masterbatch.

[0117] S4: The first masterbatch, the second masterbatch and the third masterbatch are respectively put into a single screw extruder from three hoppers, and are divided into upper, middle and lower layers by a distributor at the die head. After melt plasticization extrusion, casting, embossing, cooling, pulling and winding, a co-extruded packaging film 10 with a thickness of 0.6 mm is made, wherein the thickness of the adhesive layer 11, the ion exchange layer 12 and the anti-corrosion layer 13 are respectively 0.2 mm.

[0118] Example 2

[0119] The present embodiment differs from the embodiment 1 in that, in the ion exchange layer 12, the second matrix resin includes 10 parts by weight of acrylic resin (cation exchange resin), 90 parts by weight of a second EVA resin, and 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (third coupling agent).

[0120] That is, the weight ratio of the second EVA resin to the acrylic resin is adjusted from 8:2 to 9:1.

[0121] Example 3

[0122] The present embodiment differs from the embodiment 1 in that, in the ion exchange layer 12, the second matrix resin includes 30 parts by weight of acrylic resin (cation exchange resin), 70 parts by weight of a second EVA resin, and 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (third coupling agent).

[0123] That is, the weight ratio of the second EVA resin to the acrylic resin is adjusted from 8:2 to 7:3.

[0124] Example 4

[0125] The difference between this embodiment and embodiment 1 is that the weight ratio of the second EVA resin to the acrylic resin is adjusted from 8:2 to 5:5.

[0126] Example 5

[0127] This embodiment provides a packaging adhesive film 10, which includes an adhesive layer 11, an ion exchange layer 12 and an anti-corrosion layer 13 arranged in sequence.

[0128] The raw materials for preparing the bonding layer 11 include, by weight, 100 parts by weight of a first EVA resin, 0.8 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (a first peroxide crosslinking agent), 0.6 parts by weight of triallyl isocyanurate (a first auxiliary crosslinking agent), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a first coupling agent), 0.1 parts by weight of a vinyl silane oligomer (a coupling agent oligomer), and 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a first light stabilizer).

[0129] The raw materials for preparing the ion exchange layer 12 include, by weight, 100 parts by weight of the second matrix resin, 1.0 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (second peroxide crosslinking agent), 0.7 parts by weight of triallyl isocyanurate (second auxiliary crosslinking agent), 0.5 parts by weight of γ-methacryloxypropyl trimethoxysilane (second coupling agent), and 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (second light stabilizer). The second matrix resin includes 20 parts by weight of acrylic resin (cation exchange resin), 80 parts by weight of the second EVA resin, and 1.0 parts by weight of γ-methacryloxypropyl trimethoxysilane (third coupling agent).

[0130] In parts by weight, the raw materials for preparing the anti-corrosion layer 13 include: 100 parts by weight of a third EVA resin, 1.2 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (a third peroxide crosslinking agent), 0.6 parts by weight of a third auxiliary crosslinking agent (0.4 parts by weight of triallyl isocyanurate and 0.2 parts by weight of a tetrafunctional polyester acrylate), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a fourth coupling agent), 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a third light stabilizer), and 0.1 parts of zirconium phosphate (acid scavenger).

[0131] The preparation method of the packaging film 10 includes:

[0132] S1: pre-dissolve and mix the first co-crosslinking agent, the first coupling agent, the coupling agent oligomer and the first light stabilizer to obtain a first intermediate mixing auxiliary agent; fully stir the first EVA resin and the first peroxide, then add the first intermediate mixing auxiliary agent, and further stir and mix at a temperature of 45° C. to fully absorb the first intermediate mixing auxiliary agent to obtain a first masterbatch;

[0133] S2: The second EVA resin, the cation exchange resin and the third coupling agent are melt-mixed and extruded through a twin-screw granulator, and then cooled and pelletized to obtain a matrix masterbatch. The second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer are pre-dissolved and mixed to obtain a second intermediate mixing auxiliary agent; the matrix masterbatch and the second peroxide cross-linking agent are fully stirred and then the second intermediate mixing auxiliary agent is added, and further stirred and mixed at a temperature of 45°C to allow the second intermediate mixing auxiliary agent to be fully absorbed to obtain a second masterbatch;

[0134] S3: Pre-dissolve and mix the third co-crosslinking agent, the fourth coupling agent, the acid scavenger and the third light stabilizer to obtain a third intermediate mixing auxiliary agent; fully stir the third EVA resin and the third peroxide, then add the third intermediate mixing auxiliary agent, further stir and mix at a temperature of 45°C to allow the third intermediate mixing auxiliary agent to be fully absorbed, and obtain a third masterbatch.

[0135] S4: The first masterbatch, the second masterbatch and the third masterbatch are respectively put into a single screw extruder from three hoppers, and are divided into upper, middle and lower layers by a distributor at the die head. After melt plasticization extrusion, casting, embossing, cooling, pulling and winding, a co-extruded packaging film 10 with a thickness of 0.6 mm is made, wherein the thickness of the adhesive layer 11, the ion exchange layer 12 and the anti-corrosion layer 13 are respectively 0.2 mm.

[0136] Example 6

[0137] This embodiment provides a packaging adhesive film 10, which includes an adhesive layer 11, an ion exchange layer 12 and an anti-corrosion layer 13 arranged in sequence.

[0138] The raw materials for preparing the bonding layer 11 include, by weight, 100 parts by weight of a first EVA resin, 0.4 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (a first peroxide crosslinking agent), 0.8 parts by weight of triallyl isocyanurate (a first auxiliary crosslinking agent), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a first coupling agent), 0.4 parts by weight of vinyl silane oligomer (a coupling agent oligomer), and 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a first light stabilizer).

[0139] In terms of weight parts, the raw materials for preparing the ion exchange layer 12 include: 100 weight parts of the second base resin, 0.8 weight parts of tert-butyl peroxycarbonate-2-ethylhexyl ester (second peroxide crosslinking agent), 0.5 weight parts of triallyl isocyanurate (second auxiliary crosslinking agent), 0.4 weight parts of γ-methacryloxypropyl trimethoxysilane (second coupling agent), 0.2 weight parts of bis-2,2,6,6-tetramethylpiperidinol sebacate (second light stabilizer). Among them, the second base resin includes 20 weight parts of acrylic resin (cation exchange resin), 80 weight parts of the second EVA resin and 0.1 weight parts of γ-methacryloxypropyl trimethoxysilane (third coupling agent);

[0140] In parts by weight, the raw materials for preparing the anti-corrosion layer 13 include: 100 parts by weight of a third EVA resin, 1.0 parts by weight of tert-butyl peroxycarbonate-2-ethylhexyl ester (a third peroxide crosslinking agent), 1.0 parts by weight of a third auxiliary crosslinking agent (0.8 parts by weight of triallyl isocyanurate and 0.2 parts by weight of a tetrafunctional polyester acrylate), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a fourth coupling agent), 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a third light stabilizer), and 0.4 parts of zirconium phosphate (acid scavenger).

[0141] The preparation method of the packaging film 10 includes:

[0142] S1: pre-dissolve and mix the first co-crosslinking agent, the first coupling agent, the coupling agent oligomer and the first light stabilizer to obtain a first intermediate mixing auxiliary agent; fully stir the first EVA resin and the first peroxide, then add the first intermediate mixing auxiliary agent, and further stir and mix at a temperature of 45° C. to fully absorb the first intermediate mixing auxiliary agent to obtain a first masterbatch;

[0143] S2: The second EVA resin, the cation exchange resin and the third coupling agent are melt-mixed and extruded through a twin-screw granulator, and then cooled and pelletized to obtain a matrix masterbatch. The second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer are pre-dissolved and mixed to obtain a second intermediate mixing auxiliary agent; the matrix masterbatch and the second peroxide cross-linking agent are fully stirred and then the second intermediate mixing auxiliary agent is added, and further stirred and mixed at a temperature of 45°C to allow the second intermediate mixing auxiliary agent to be fully absorbed to obtain a second masterbatch;

[0144] S3: Pre-dissolve and mix the third co-crosslinking agent, the fourth coupling agent, the acid scavenger and the third light stabilizer to obtain a third intermediate mixing auxiliary agent; fully stir the third EVA resin and the third peroxide, then add the third intermediate mixing auxiliary agent, further stir and mix at a temperature of 45°C to allow the third intermediate mixing auxiliary agent to be fully absorbed, and obtain a third masterbatch.

[0145] S4: The first masterbatch, the second masterbatch and the third masterbatch are respectively put into a single screw extruder from three hoppers, and are divided into upper, middle and lower layers by a distributor at the die head. After melt plasticization extrusion, casting, embossing, cooling, pulling and winding, a co-extruded packaging film 10 with a thickness of 0.6 mm is made, wherein the thickness of the adhesive layer 11, the ion exchange layer 12 and the anti-corrosion layer 13 are respectively 0.2 mm.

[0146] Example 7

[0147] This embodiment provides a packaging adhesive film 10, which includes an adhesive layer 11, an ion exchange layer 12 and an anti-corrosion layer 13 arranged in sequence.

[0148] The raw materials for preparing the bonding layer 11 include, by weight, 100 parts by weight of a first EVA resin, 0.5 parts by weight of tert-amyl peroxide (2-ethylhexyl) carbonate (a first peroxide crosslinking agent), 0.5 parts by weight of trimethylolpropane trimethacrylate (a first auxiliary crosslinking agent), 0.1 parts by weight of vinyltrimethoxysilane (a first coupling agent), 0.4 parts by weight of a bisamino coupling agent oligomer (a coupling agent oligomer), and 0.2 parts by weight of poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate (a first light stabilizer).

[0149] In terms of weight parts, the raw materials for preparing the ion exchange layer 12 include: 100 weight parts of the second base resin, 0.5 weight parts of tert-butyl peroxyacetate (second peroxide crosslinking agent), 0.5 weight parts of trimethylolpropane triethoxy acrylate (second auxiliary crosslinking agent), 0.1 weight parts of vinyl tri(β-methoxyethoxy) silane (second coupling agent), 0.2 weight parts of sebacate bis-2,2,6,6-tetramethylpiperidinol ester (second light stabilizer). Among them, the second base resin includes 20 weight parts of acrylic resin (cation exchange resin), 80 weight parts of the second EVA resin, 0.1 weight parts of oxyacrylate (second auxiliary crosslinking agent), and 0.1 weight parts of (third coupling agent);

[0150] In parts by weight, the raw materials for preparing the anti-corrosion layer 13 include: 100 parts by weight of a third EVA resin, 0.8 parts by weight of tert-butyl peroxide-2-ethylhexanoate (a third peroxide crosslinking agent), 0.9 parts by weight of a third auxiliary crosslinking agent (0.6 parts by weight of ethoxylated trimethylolpropane triacrylate and 0.3 parts by weight of 1,6-hexanediol diacrylate), 0.4 parts by weight of γ-methacryloxypropyltrimethoxysilane (a fourth coupling agent), 0.2 parts by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a third light stabilizer), and 0.01 parts of magnesium oxide (acid scavenger).

[0151] The preparation method of the packaging film 10 includes:

[0152] S1: pre-dissolve and mix the first co-crosslinking agent, the first coupling agent, the coupling agent oligomer and the first light stabilizer to obtain a first intermediate mixing auxiliary agent; fully stir the first EVA resin and the first peroxide, then add the first intermediate mixing auxiliary agent, and further stir and mix at a temperature of 40° C. to fully absorb the first intermediate mixing auxiliary agent to obtain a first masterbatch;

[0153] S2: The second EVA resin, the cation exchange resin and the third coupling agent are melt-mixed and extruded through a twin-screw granulator, and then cooled and pelletized to obtain a matrix masterbatch. The second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer are pre-dissolved and mixed to obtain a second intermediate mixing aid; the matrix masterbatch and the second peroxide cross-linking agent are fully stirred and then the second intermediate mixing aid is added, and further stirred and mixed at a temperature of 40°C to allow the second intermediate mixing aid to be fully absorbed to obtain a second masterbatch;

[0154] S3: Pre-dissolve and mix the third cross-linking agent, the fourth coupling agent, the acid scavenger and the third light stabilizer to obtain a third intermediate mixing auxiliary agent; fully stir the third EVA resin and the third peroxide, then add the third intermediate mixing auxiliary agent, further stir and mix at a temperature of 40°C to allow the third intermediate mixing auxiliary agent to be fully absorbed, and obtain a third masterbatch.

[0155] S4: The first masterbatch, the second masterbatch and the third masterbatch are respectively put into a single screw extruder from three hoppers, and are divided into upper, middle and lower layers by a distributor at the die head. After melt plasticization extrusion, casting, embossing, cooling, pulling and winding, a co-extruded packaging film 10 with a thickness of 0.9 mm is made, wherein the thickness of the adhesive layer 11, the ion exchange layer 12 and the anti-corrosion layer 13 are respectively 0.3 mm.

[0156] Example 8

[0157] This embodiment provides a packaging adhesive film 10, which includes an adhesive layer 11, an ion exchange layer 12 and an anti-corrosion layer 13 arranged in sequence.

[0158] The raw materials for preparing the bonding layer 11 include, by weight, 100 parts by weight of a first EVA resin, 2 parts by weight of tert-butyl peroxybenzoate (a first peroxide crosslinking agent), 2 parts by weight of trimethylolpropane triacrylate (a first auxiliary crosslinking agent), 2 parts by weight of vinyl triethoxysilane (a first coupling agent), 2 parts by weight of an epoxy coupling agent oligomer (a coupling agent oligomer), and 1 part by weight of bis(2,2,6,6-tetramethyl-4-piperidinol) sebacic acid ester (a first light stabilizer).

[0159] The raw materials for preparing the ion exchange layer 12 include, by weight, 20 parts of the second matrix resin, 2 parts of tert-amyl peroxide-2-ethylhexanoate (second peroxide crosslinking agent), 2 parts of triallyl isocyanate (second auxiliary crosslinking agent), 2 parts of vinyl tri-tert-butyloxysilane (second coupling agent), and 1 part of bis-2,2,6,6-tetramethylpiperidinol sebacate (second light stabilizer). The second matrix resin includes 20 parts of acrylic resin (cation exchange resin), 80 parts of the second EVA resin, and 2 parts of vinyl tri-tert-butyloxysilane (third coupling agent).

[0160] In parts by weight, the raw materials for preparing the anti-corrosion layer 13 include: 100 parts by weight of a third EVA resin, 2 parts by weight of diisopropylbenzene peroxide (a third peroxide crosslinking agent), 2 parts by weight of a third auxiliary crosslinking agent (0.6 parts by weight of propoxylated glycerol triacrylate and 0.3 parts by weight of a tetrafunctional polyester acrylate), 2 parts by weight of γ-methacryloxypropyltrimethoxysilane (a fourth coupling agent), 1 part by weight of bis-2,2,6,6-tetramethylpiperidinol sebacate (a third light stabilizer), and 1 part of calcium stearate (acid scavenger).

[0161] The preparation method of the packaging film 10 includes:

[0162] S1: pre-dissolve and mix the first co-crosslinking agent, the first coupling agent, the coupling agent oligomer and the first light stabilizer to obtain a first intermediate mixing auxiliary agent; fully stir the first EVA resin and the first peroxide, then add the first intermediate mixing auxiliary agent, and further stir and mix at a temperature of 50° C. to fully absorb the first intermediate mixing auxiliary agent to obtain a first masterbatch;

[0163] S2: The second EVA resin, the cation exchange resin and the third coupling agent are melt-mixed and extruded through a twin-screw granulator, and then cooled and pelletized to obtain a base masterbatch. The second auxiliary cross-linking agent, the second coupling agent and the second light stabilizer are pre-dissolved and mixed to obtain a second intermediate mixing aid; the base masterbatch and the second peroxide cross-linking agent are fully stirred and then the second intermediate mixing aid is added, and further stirred and mixed at a temperature of 50°C to allow the second intermediate mixing aid to be fully absorbed to obtain a second masterbatch;

[0164] S3: Pre-dissolve and mix the third co-crosslinking agent, the fourth coupling agent, the acid scavenger and the third light stabilizer to obtain a third intermediate mixing auxiliary agent; fully stir the third EVA resin and the third peroxide, then add the third intermediate mixing auxiliary agent, further stir and mix at a temperature of 50°C to allow the third intermediate mixing auxiliary agent to be fully absorbed, and obtain a third masterbatch.

[0165] S4: The first masterbatch, the second masterbatch and the third masterbatch are respectively put into a single screw extruder from three hoppers, and are divided into upper, middle and lower layers by a distributor at the die head. After melt plasticization extrusion, casting, embossing, cooling, pulling and winding, a co-extruded packaging film 10 with a thickness of 1.8 mm is made, wherein the thickness of the adhesive layer 11, the ion exchange layer 12 and the anti-corrosion layer 13 are respectively 0.6 mm.

[0166] Example 9

[0167] The difference between this embodiment and embodiment 1 is that the second matrix resin of the ion exchange layer 12 does not contain EVA resin.

[0168] Comparative Example 1

[0169] The difference between this comparative example and Example 1 is that the packaging film 10 is composed of only two layers, the adhesive layer 11 and the ion exchange layer 12, and the thickness of the adhesive layer 11 and the ion exchange layer 12 are both 0.3 mm.

[0170] Comparative Example 2

[0171] The difference between this comparative example and Example 1 is that the packaging film 10 is composed of only two layers, the adhesive layer 11 and the anti-corrosion layer 13 , and the thickness of the adhesive layer 11 and the anti-corrosion layer 13 are both 0.3 mm.

[0172] Comparative Example 3

[0173] The difference between this comparative example and Example 1 is that the packaging film 10 is composed of only two layers, the ion exchange layer 12 and the anti-corrosion layer 13 , and the thickness of the ion exchange layer 12 and the anti-corrosion layer 13 are both 0.3 mm.

[0174] Comparative Example 4

[0175] The difference between this embodiment and embodiment 1 is that the raw materials for preparing the bonding layer 11 do not contain coupling agent oligomers.

[0176] Comparative Example 5

[0177] The difference between this embodiment and embodiment 1 is that the raw material for preparing the anti-corrosion layer 13 does not contain an acid scavenger.

[0178] Comparative Example 6

[0179] The difference between this embodiment and embodiment 1 is that the auxiliary cross-linking agent in the anti-corrosion layer does not contain tetrafunctional polyester acrylate.

[0180] Comparative Example 7

[0181] The difference between this embodiment and embodiment 1 is that the cation exchange resin in the ion exchange layer 12 is replaced by a sulfonic acid cation exchange resin (specifically 2-acrylamide-2-methylpropane sulfonic acid resin) instead of acrylic acid resin.

[0182] Comparative Example 8

[0183] The difference between this embodiment and embodiment 1 is that the cation exchange resin in the ion exchange layer 12 is replaced by a phenol-based cation exchange resin (specifically, a salicylic acid resin) instead of an acrylic acid resin.

[0184] Test example

[0185] The films in the above-mentioned Examples 1 to 9 and Comparative Examples 1 to 8 were respectively prepared into test samples in the following manner (such as Figure 2 As shown in the figure): from bottom to top, the first glass layer 21, the first encapsulation film layer 22, the battery cell 23, the second encapsulation film layer 24 and the second glass layer 25 are arranged in sequence; wherein, the encapsulation film 10 used in the first encapsulation film layer 22 and the second encapsulation film layer 24 are the same, and are both the encapsulation films 10 provided in the embodiment to be tested or the comparative example to be tested. After being laid in the above order, heating and lamination are performed to form the sample to be tested, wherein the lamination process parameters are temperature 148°C, vacuum 6min, pressurization 1min, and pressure holding 12min.

[0186] The performance test of the sample to be tested is carried out, and the results are as follows Figure 1 As shown. Among them, the water vapor transmission rate is tested in accordance with GB / T29848-2018, and the wavelength test range is 380nm~1100nm; the peel strength is tested in accordance with GB / T29848-2018; the power attenuation is tested in accordance with GB / T29848-2018. Among them, "DH2000" refers to the result corresponding to the relative humidity of 85%, the temperature of 85℃, and aging for 2000h; "PID192" refers to the result corresponding to the test sample after it is powered on, works at a voltage of -1500V for 192h, and the relative humidity of the external environment is 85%, the temperature is 85℃, and aging for 2000h.

[0187] Table 1 Performance test results

[0188]

[0189] It can be seen from Table 1 that the encapsulation films 10 provided in Examples 1 to 9 of the present invention can enable the corresponding solar cell modules to obtain lower water vapor transmission rate, higher peel strength and lower power attenuation.

[0190] It can be seen from Example 1 and Comparative Examples 1 to 8 that if the layer structure of the encapsulation film 10 is improperly set or the raw materials for preparing the encapsulation film 10 are improperly selected, the corresponding solar cell module will not be able to simultaneously obtain better water vapor transmission, higher peel strength and lower power attenuation.

[0191] Among them, it can be seen from Example 1 and Comparative Example 4 that the use of vinyl silane oligomers (coupling agent oligomers) has an impact on the performance of solar cell modules. The reason may be that vinyl silane oligomers (coupling agent oligomers) can provide long-lasting adhesion in DH2000 wet heat aging, the silane bond formed by vinyl silane oligomers and glass is not easily hydrolyzed, and the side chain vinyl is hydrophobic and has a certain barrier effect on water vapor.

[0192] It can be seen from Example 1 and Comparative Example 5 that the use of acid scavengers has an impact on the performance of solar cell modules. The reason may be that the acid scavengers in the anti-corrosion layer 13 can neutralize the acid precipitated in the EVA film, prevent the corrosion of the silver paste of the battery cell 23, and ensure the long-term stability of the module power.

[0193] It can be seen from Example 1 and Comparative Example 6 that the use of a co-crosslinking agent has an impact on the performance of solar cell modules. The reason may be that the use of a tetrafunctional polyester acrylate as a co-crosslinking agent can enhance the crosslinking speed and crosslinking density of the EVA film, and improve the volume resistivity and water barrier properties of the film.

[0194] It can be seen from Example 1 and Comparative Examples 7-8 that the acrylic resin in the ion exchange layer 12 plays a key role in the aging process of PID192. The acrylic resin absorbs the sodium ions migrating from the glass side and prevents the sodium ions from corroding the battery cell 23.

[0195] In summary, the packaging film 10 with a specific structure prepared from the specific raw materials provided by the present invention has good adhesion and corrosion resistance, can reduce the power attenuation of solar cells, and broaden the application scope of the EVA packaging film 10 in the market.

[0196] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A packaging film, characterized in that: The packaging film comprises an adhesive layer, an ion exchange layer and an anti-corrosion layer arranged in sequence; The first base resin of the bonding layer is a first EVA resin; The second matrix resin of the ion exchange layer includes a cation exchange resin; wherein the cation exchange resin includes an acrylic resin; The third base resin of the anti-corrosion layer is a third EVA resin; The second matrix resin further comprises a second EVA resin, and the weight ratio of the second EVA resin to the cation exchange resin is 9:1 to 7:3; The raw materials for preparing the bonding layer include, by weight: 100 parts of a first base resin, 0.1 to 2 parts of a first peroxide crosslinking agent, 0.1 to 2 parts of a first auxiliary crosslinking agent, 0.1 to 2 parts of a first coupling agent, 0.1 to 2 parts of a coupling agent oligomer, and 0.01 to 1 parts of a first light stabilizer; The raw materials for preparing the ion exchange layer include, by weight: 20 to 100 parts of a second base resin, 0.1 to 2 parts of a second peroxide crosslinking agent, 0.1 to 2 parts of a second auxiliary crosslinking agent, 0.1 to 2 parts of a second coupling agent, and 0.01 to 1 parts of a second light stabilizer; The raw materials for preparing the anti-corrosion layer include, by weight: 100 parts of a third base resin, 0.1 to 2 parts of a third peroxide cross-linking agent, 0.1 to 2 parts of a third auxiliary cross-linking agent, 0.1 to 2 parts of a fourth coupling agent, 0.01 to 1 parts of an acid scavenger, and 0.01 to 1 parts of a third light stabilizer; The third auxiliary cross-linking agent includes tetrafunctional polyester acrylate.

2. The packaging film according to claim 1, characterized in that: The first co-crosslinking agent and the second co-crosslinking agent independently include at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane triethoxyacrylate, triallyl isocyanate, ethoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate, tetrafunctional polyester acrylate and 1,6-hexanediol diacrylate; the third co-crosslinking agent also includes at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane triethoxyacrylate, triallyl isocyanate, ethoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate and 1,6-hexanediol diacrylate; Or, the coupling agent oligomer includes at least one of a vinyl coupling agent oligomer, a bisamino coupling agent oligomer, an epoxy coupling agent oligomer, an alkoxy coupling agent oligomer and a methacryloxy coupling agent oligomer; Alternatively, the acid scavenger includes at least one of magnesium oxide, magnesium hydroxide, magnesium silicate, hydrotalcite, silicon dioxide, calcium stearate, zinc oxide and zirconium phosphate.

3. The packaging film according to claim 2, characterized in that: In parts by weight, the second base resin includes 5 to 100 parts of a second EVA resin, more than 0 and no more than 100 parts of a cation exchange resin, and 0.1 to 2 parts of a third coupling agent.

4. The packaging film according to claim 3, characterized in that: The first peroxide crosslinking agent, the second peroxide crosslinking agent and the third peroxide crosslinking agent independently include at least one of tert-butyl peroxycarbonate-2-ethylhexyl, tert-amyl peroxy (2-ethylhexyl) carbonate, tert-butyl peroxybenzoate, tert-butyl peroxyacetate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate and dicumyl peroxide; Or, the first coupling agent, the second coupling agent, the third coupling agent, the third coupling agent and the fourth coupling agent independently include at least one of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl tri (β-methoxyethoxy) silane, γ-methacryloxypropyl trimethoxy silane and vinyl tri-tert-butoxy silane; Alternatively, the first light stabilizer, the second light stabilizer and the third light stabilizer are independently hindered amine light stabilizers.

5. The packaging film according to claim 1, characterized in that: The thickness of the bonding layer is 0.10 mm to 0.60 mm; or the thickness of the ion exchange layer is 0.10 mm to 0.60 mm; or the thickness of the anti-corrosion layer is 0.10 mm to 0.60 mm.

6. A method for preparing a packaging film according to any one of claims 1 to 5, characterized in that: The following steps are involved: The first masterbatch prepared from the raw material for preparing the bonding layer, the second masterbatch prepared from the raw material for preparing the ion exchange layer, and the third masterbatch prepared from the raw material for preparing the anti-corrosion layer are subjected to extrusion, casting and calendering.

7. A solar cell module, characterized in that: The solar cell module comprises the encapsulation film according to any one of claims 1 to 5.

8. The solar cell assembly according to claim 7, characterized in that: The solar cell assembly comprises a first glass layer, a first packaging film layer, a battery cell, a second packaging film layer and a second glass layer arranged in sequence from bottom to top; Wherein, the encapsulation films in the first encapsulation film layer and the second encapsulation film layer are both the encapsulation films according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Photovoltaic module containing multilayer packaging adhesive film and preparation method thereof

    CN111863996A

  • Multifunctional packaging adhesive film and preparation method thereof

    CN111961422A

  • Colored adhesive film, preparation method thereof and colored solar photovoltaic module

    CN113956801A

  • High-reflection black adhesive film as well as preparation method and application thereof

    CN114149769A

  • High-water-resistance EVA (Ethylene Vinyl Acetate) adhesive film for packaging solar cell and preparation method thereof

    CN114774007A