Conductive copper slurry and preparation method thereof
By using raw materials such as copper powder, composite functional agents and nano-silica to prepare conductive copper slurry, the problem of poor heat resistance of epoxy resin and easy oxidation of copper powder is solved, achieving low cost, high thermal stability and oxidation resistance. Conductive copper paste expands its application scenarios.
Patent Information
- Application Number
- CN202411082115.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The organic carrier epoxy resin of the conductive copper slurry has poor heat resistance, which affects its stability, and the copper powder is easily oxidized. The existing technology uses silver-coated copper, but the cost is high, which limits its application scenarios.
Conductive copper slurry is prepared using copper powder, composite functional agent, nano-silica and organic carrier, and is coated with composite functional agent through pickling, ethanol washing and heat treatment to prevent oxidation of copper powder, and use composite functional agent to improve nano-silica slurry. The dispersion and wettability of silicon in epoxy resin improve the thermal stability and mechanical properties of conductive copper paste.
It significantly reduces production costs, improves the oxidation resistance and thermal stability of conductive copper paste, and maintains good stability at high temperatures. It is suitable for circuit boards, electronic components, flat panel displays and other fields.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic pastes, and in particular, relates to a conductive copper paste and a preparation method thereof. Background Art
[0002] Conductive copper paste is a conductive material with copper powder as the main raw material. Its preparation process is relatively simple, and its production cost is low, with a high cost performance ratio. Conductive copper paste has various processing methods and a wide range of application scenarios. These advantages make conductive copper paste widely used in the electronics industry.
[0003] However, because the organic carrier of the conductive copper paste is usually epoxy resin, and epoxy resin has poor heat resistance, the internal structure of the epoxy resin may change under high temperature conditions for a long time, thereby affecting the resistance of the cured product. Therefore, the stability of the conductive copper paste is easily affected by temperature, which makes the conductive copper paste unable to be used in a high temperature environment, severely limiting the application scenarios of the conductive copper paste; in addition, the copper powder in the conductive copper paste is not stable and is easily oxidized by air. Silver-coated copper is often used in the prior art to solve the problem of easy oxidation of copper powder, but silver is expensive and its price is still rising, which is not conducive to promotion. Summary of the invention
[0004] The object of the present invention is to provide a conductive copper paste and a preparation method thereof, so as to solve the problems in the above-mentioned background technology.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A conductive copper slurry comprises the following raw materials in parts by weight: 65-75 parts of copper powder, 8-10 parts of a composite functional agent, 5-8 parts of nano silicon dioxide, 15-25 parts of an organic carrier, and 1-3 parts of a cross-linking agent.
[0007] A method for preparing a conductive copper slurry comprises the following steps:
[0008] Step 1: Weigh and screen each raw material according to mass fraction;
[0009] Step 2: After the copper powder is acid-washed and ethanol-washed, it is stirred and mixed with the composite functional agent, and heat-treated to obtain the copper powder coated with the composite functional agent;
[0010] Step 3: Fully mix the copper powder coated with the composite functional agent, nano silicon dioxide, an organic carrier, and a cross-linking agent to obtain the conductive copper slurry;
[0011] Furthermore, the particle size of the copper powder is 100nm-3μm.
[0012] Furthermore, in the second step, the acid used for pickling is 15% by mass hydrochloric acid, the ethanol used for ethanol washing is 98% by mass industrial ethanol, the temperature condition of heat treatment is 55-65° C., and the time condition of heat treatment is 90-120 min.
[0013] Furthermore, in the third step, the mixing temperature condition is 35-45° C., and the mixing time condition is 30-45 min.
[0014] Furthermore, the organic carrier is glycidylamine epoxy resin.
[0015] Furthermore, the cross-linking agent is one of phthalic acid and terephthalic acid.
[0016] Furthermore, the composite functional agent is prepared by the following steps:
[0017] Step 1: maleic anhydride and ethyl acetate are added to a three-necked flask, and the three-necked flask is placed in an ice-water bath environment, and the p-aminophenol solution is added dropwise to the three-necked flask. After the addition is completed, the ice-water bath is removed, stirred, and filtered, and the filtered product, cyanuric chloride, tetrahydrofuran, and triethylamine are added to the three-necked flask, and magnetic stirring is turned on. The reaction is carried out under ice-water bath conditions for 3 hours. After the reaction is completed, the mixture is washed with a sodium bicarbonate solution, and the organic layer is separated by a separatory funnel, dried, filtered, and rotated to obtain intermediate 1;
[0018] Step 2: Add intermediate 1, triethylsilyl hydride and phosphonium cation solution into a three-necked flask, react at 60°C for 4 hours, and after the reaction, rotary evaporate to obtain intermediate 2;
[0019] Step 3: Add sodium hydroxide solution and dichloromethane solution of intermediate 2 into a three-necked flask, turn on magnetic stirring, add dichloromethane solution of phosphorus oxychloride into the three-necked flask, react at room temperature for 2.5 hours, after the reaction is completed, add sodium hydroxide solution to the three-necked flask for washing, separate the organic layer with a separatory funnel, wash with saturated sodium chloride solution until neutral, dry, and obtain the composite functional agent after rotary evaporation.
[0020] Furthermore, the p-aminophenol solution in step 1 is prepared from 0.1 mol of p-aminophenol and 30-36 g of ethyl acetate, and the amount ratio of maleic anhydride, ethyl acetate, p-aminophenol solution, cyanuric chloride, tetrahydrofuran and triethylamine used is 0.1 mol: 220-240 g: 41-47 g: 18-20 g: 72-80 g: 24-30 g.
[0021] Furthermore, the phosphonium cation solution in step 2 is prepared from 1 g of [(C6F5)3PF][B(C6F5)4] and 150-180 g of dichloromethane, and the dosage ratio of intermediate 1, triethylsilyl hydride and phosphonium cation solution is 0.08 mol: 0.08-0.1 mol: 151-181 g.
[0022] Furthermore, the sodium hydroxide solution in step 3 is prepared from 1.5 g of sodium hydroxide and 5 g of ultrapure water, the dichloromethane solution of intermediate 2 is prepared from 0.06 mol of intermediate 2 and 40 g of dichloromethane, and the dichloromethane solution of phosphorus oxychloride is prepared from 0.02 mol of phosphorus oxychloride and 15 g of dichloromethane, and the amount ratio of the sodium hydroxide solution, the dichloromethane solution of intermediate 2, and the dichloromethane solution of phosphorus oxychloride is 6.5 g:58.3 g:18 g.
[0023] Beneficial effects of the present invention:
[0024] The present invention uses copper powder, composite functional agent, nano silicon dioxide, organic carrier and cross-linking agent as raw materials to prepare a conductive copper slurry. The conductive copper slurry preparation process of the present invention is simple, and no silver is used in the processing process, which significantly reduces the production cost.
[0025] The present invention uses maleic anhydride and p-aminophenol as raw materials, cyanuric chloride as a catalyst, and triethylamine as an acid-binding agent to prepare an intermediate 1 with a rigid structure, and then the double bond of the intermediate 1 and triethylsilyl hydride undergo addition reaction under the catalytic action of phosphonium cations to obtain an intermediate 2 with an organosilicon structure, and finally the intermediate 2 and phosphorus oxychloride undergo nucleophilic substitution reaction to obtain a composite functional agent with a phosphate structure, and the composite functional agent is used to perform organic phosphating treatment on copper powder, so that a complex layer can be formed on the surface of the copper powder to prevent copper from contacting with oxygen atoms, thereby preventing the copper powder from being oxidized. In addition, the composite functional agent has both an organic-philic structure and an inorganic-philic structure (organosilicon structure), which can improve the dispersibility and wettability of nano-silicon dioxide in epoxy resin, and improve the overall heat resistance and mechanical properties of the conductive copper slurry. The rigid structural group in the composite functional agent can also significantly improve the internal rotation resistance of the molecular chain, and synergistically improve the thermal stability of the conductive copper slurry.
[0026] The conductive copper paste of the present invention has good thermal stability after curing and strong oxidation resistance. The resistance will not change significantly when placed at room temperature for a long time, and can still maintain good stability at higher temperatures. It can be widely used in circuit boards, electronic components, flat panel displays and touch control fields. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A composite functional agent is prepared by the following steps
[0030] Step 1: 0.1 mol of maleic anhydride and 220 g of ethyl acetate are added to a container, and the container is placed in an ice-water bath environment, 41 g of p-aminophenol solution is added to the container, and after the addition is completed, the ice-water bath is removed, stirred, and filtered, and the filtered product and 18 g of cyanuric chloride, 72 g of tetrahydrofuran, and 24 g of triethylamine are added to the container, and reacted for 3 hours under ice-water bath conditions. After the reaction is completed, the product is washed with a sodium bicarbonate solution, and the organic layer is separated by a separatory funnel, dried, filtered, and rotated to obtain an intermediate 1. The p-aminophenol solution used is prepared from 0.1 mol of p-aminophenol and 30 g of ethyl acetate;
[0031] Step 2: 0.08 mol of intermediate 1, 0.08 mol of triethylsilyl hydride, and 151 g of phosphonium cation solution were added into a container, and reacted at 60° C. for 4 h. After the reaction, intermediate 2 was obtained by rotary evaporation. The phosphonium cation solution was prepared by 1 g of [(C6F5)3PF][B(C6F5)4] and 150 g of dichloromethane;
[0032] Step 3: Add 6.5g of sodium hydroxide solution and 58.3g of dichloromethane solution of intermediate 2 into a container, turn on magnetic stirring, add 18g of dichloromethane solution of phosphorus oxychloride into the container, react at room temperature for 2.5h, after the reaction is completed, add sodium hydroxide solution to the container for washing, separate the organic layer with a separatory funnel, wash with saturated sodium chloride solution until neutral, dry, and rotary evaporate to obtain the composite functional agent, the sodium hydroxide solution used is prepared from 1.5g of sodium hydroxide and 5g of ultrapure water, the dichloromethane solution of intermediate 2 is prepared from 0.06mol of intermediate 2 and 40g of dichloromethane, and the dichloromethane solution of phosphorus oxychloride is prepared from 0.02mol of phosphorus oxychloride and 15g of dichloromethane.
[0033] Example 2
[0034] A composite functional agent is prepared by the following steps
[0035] Step 1: 0.1 mol of maleic anhydride and 230 g of ethyl acetate are added to a container, and the container is placed in an ice-water bath environment, 44 g of p-aminophenol solution is added to the container, and after the addition is completed, the ice-water bath is removed, stirred, and filtered, and the filtered product and 19 g of cyanuric chloride, 76 g of tetrahydrofuran, and 27 g of triethylamine are added to the container, and reacted for 3 hours under ice-water bath conditions. After the reaction is completed, the product is washed with a sodium bicarbonate solution, and the organic layer is separated by a separatory funnel, dried, filtered, and rotated to obtain an intermediate 1. The p-aminophenol solution used is prepared from 0.1 mol of p-aminophenol and 33 g of ethyl acetate;
[0036] Step 2: 0.08 mol of intermediate 1, 0.09 mol of triethylsilyl hydride, and 166 g of phosphonium cation solution were added into a container, and reacted at 60°C for 4 h. After the reaction, intermediate 2 was obtained by rotary evaporation. The phosphonium cation solution was prepared by 1 g of [(C6F5)3PF][B(C6F5)4] and 165 g of dichloromethane;
[0037] Step 3: Add 6.5g of sodium hydroxide solution and 58.3g of dichloromethane solution of intermediate 2 into a container, turn on magnetic stirring, add 18g of dichloromethane solution of phosphorus oxychloride into the container, react at room temperature for 2.5h, after the reaction is completed, add sodium hydroxide solution to the container for washing, separate the organic layer with a separatory funnel, wash with saturated sodium chloride solution until neutral, dry, and rotary evaporate to obtain the composite functional agent, the sodium hydroxide solution used is prepared from 1.5g of sodium hydroxide and 5g of ultrapure water, the dichloromethane solution of intermediate 2 is prepared from 0.06mol of intermediate 2 and 40g of dichloromethane, and the dichloromethane solution of phosphorus oxychloride is prepared from 0.02mol of phosphorus oxychloride and 15g of dichloromethane.
[0038] Example 3
[0039] A composite functional agent is prepared by the following steps
[0040] Step 1: 0.1 mol of maleic anhydride and 240 g of ethyl acetate are added to a container, and the container is placed in an ice-water bath environment, 47 g of p-aminophenol solution is added to the container, and after the addition is completed, the ice-water bath is removed, stirred, and filtered, and the filtered product and 20 g of cyanuric chloride, 80 g of tetrahydrofuran, and 30 g of triethylamine are added to the container, and reacted for 3 hours under ice-water bath conditions. After the reaction is completed, the product is washed with a sodium bicarbonate solution, and the organic layer is separated by a separatory funnel, dried, filtered, and rotated to obtain an intermediate 1. The p-aminophenol solution used is prepared from 0.1 mol of p-aminophenol and 36 g of ethyl acetate;
[0041] Step 2: 0.08 mol of intermediate 1, 0.1 mol of triethylsilyl hydride, and 181 g of phosphonium cation solution were added into a container, and reacted at 60°C for 4 h. After the reaction, intermediate 2 was obtained by rotary evaporation. The phosphonium cation solution was prepared by 1 g of [(C6F5)3PF][B(C6F5)4] and 180 g of dichloromethane;
[0042] Step 3: Add 6.5g of sodium hydroxide solution and 58.3g of dichloromethane solution of intermediate 2 into a container, turn on magnetic stirring, add 18g of dichloromethane solution of phosphorus oxychloride into the container, react at room temperature for 2.5h, after the reaction is completed, add sodium hydroxide solution to the container for washing, separate the organic layer with a separatory funnel, wash with saturated sodium chloride solution until neutral, dry, and rotary evaporate to obtain the composite functional agent, the sodium hydroxide solution used is prepared from 1.5g of sodium hydroxide and 5g of ultrapure water, the dichloromethane solution of intermediate 2 is prepared from 0.06mol of intermediate 2 and 40g of dichloromethane, and the dichloromethane solution of phosphorus oxychloride is prepared from 0.02mol of phosphorus oxychloride and 15g of dichloromethane.
[0043] Experimental Example 1
[0044] The composite functional agent obtained in Examples 1-3 and the copper powder were heat treated to obtain copper powder coated with the composite functional agent. The three groups of copper powder coated with the composite functional agent were placed together in a vacuum drying oven, and another group of untreated copper powder of the same amount was placed as a blank control. They were placed at 160° C. for 300 minutes, and the oxygen content at each stage was tested with an oxygen content tester. The test results are shown in Table 1:
[0045] Table 1
[0046]
[0047] It can be seen from Table 1 that the oxidation resistance of the copper powder after heat treatment with the composite functional agent prepared in Examples 1-3 is greatly improved compared with the untreated copper powder, indicating that the composite functional agent of the present invention can effectively improve the oxidation resistance of the copper powder.
[0048] Example 4
[0049] A conductive copper paste comprises the following raw materials in parts by mass: 65 parts of copper powder with a particle size of 100 nm-3 μm, 8 parts of the composite functional agent prepared in Example 1, 5 parts of nano silicon dioxide, 15 parts of glycidylamine epoxy resin, and 1 part of terephthalic acid.
[0050] A method for preparing a conductive copper slurry comprises the following steps:
[0051] Step 1: Weigh and screen each raw material according to mass fraction;
[0052] Step 2: After the copper powder is acid-washed and ethanol-washed, it is stirred and mixed with the composite functional agent, and heat-treated at 55°C for 90 minutes to obtain copper powder coated with the composite functional agent;
[0053] Step 3: Fully mix the copper powder coated with the composite functional agent, nano silicon dioxide, organic carrier and cross-linking agent at a temperature of 35° C. for 30 minutes to obtain the conductive copper slurry.
[0054] Example 5
[0055] A conductive copper slurry comprises the following raw materials in parts by mass: 75 parts of copper powder with a particle size of 100 nm-3 μm, 10 parts of the composite functional agent prepared in Example 2, 8 parts of nano silicon dioxide, 15 parts of glycidylamine epoxy resin, and 1 part of phthalic acid.
[0056] A method for preparing a conductive copper slurry comprises the following steps:
[0057] Step 1: Weigh and screen each raw material according to mass fraction;
[0058] Step 2: After the copper powder is acid-washed and ethanol-washed, it is stirred and mixed with the composite functional agent, and heat-treated at 55°C for 90 minutes to obtain copper powder coated with the composite functional agent;
[0059] Step 3: Fully mix the copper powder coated with the composite functional agent, nano silicon dioxide, organic carrier and cross-linking agent at a temperature of 35° C. for 30 minutes to obtain the conductive copper slurry.
[0060] Example 6
[0061] A conductive copper paste comprises the following raw materials in parts by mass: 65 parts of copper powder with a particle size of 100 nm-3 μm, 8 parts of the composite functional agent prepared in Example 3, 5 parts of nano silicon dioxide, 25 parts of glycidylamine epoxy resin, and 3 parts of terephthalic acid.
[0062] A method for preparing a conductive copper slurry comprises the following steps:
[0063] Step 1: Weigh and screen each raw material according to mass fraction;
[0064] Step 2: After the copper powder is acid-washed and ethanol-washed, it is stirred and mixed with the composite functional agent, and heat-treated at 55°C for 90 minutes to obtain copper powder coated with the composite functional agent;
[0065] Step 3: Fully mix the copper powder coated with the composite functional agent, nano silicon dioxide, organic carrier and cross-linking agent at a temperature of 35° C. for 30 minutes to obtain the conductive copper slurry.
[0066] Comparative Example 1
[0067] The second step in Example 6 was removed, and the copper powder coated with the composite functional agent in the third step was replaced with untreated copper powder, and the other steps remained unchanged.
[0068] Comparative Example 2
[0069] This comparative example is the conductive copper paste sold by Shenzhen Yilai Technology Co., Ltd.
[0070] The conductive copper pastes of Examples 4-6 and Comparative Examples 1-2 were cured, and the square resistance of the cured samples was tested. The cured samples were placed at room temperature for 6 months, and then their square resistance was measured again. Finally, the cured samples were heated at 160° C. for 60 min, and their resistance changes were tested. The test results are shown in Table 2:
[0071] Table 2
[0072]
[0073] It can be seen from Table 2 that the sheet resistance of the conductive copper slurries prepared in Examples 4-6 after curing is significantly lower than that of Comparative Examples 1-2, and the resistance is little affected by long-term storage at room temperature, and the resistance does not change significantly under the influence of high temperature for a long time, showing excellent thermal stability. Therefore, it can be widely used in circuit boards, electronic components, flat panel displays and touch screens.
[0074] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A conductive copper paste, characterized in that: The method comprises the following raw materials in parts by weight: 65-75 parts of copper powder, 8-10 parts of composite functional agent, 5-8 parts of nano silicon dioxide, 15-25 parts of organic carrier, and 1-3 parts of cross-linking agent; Wherein, the composite functional agent is prepared by the following steps: Step 1, maleic anhydride and ethyl acetate are added to a container, and the container is placed in an ice-water bath environment, and p-aminophenol solution is added to the container. After the addition is completed, the ice-water bath is removed, and the filtered product and cyanuric chloride, tetrahydrofuran, and triethylamine are added to the container, and the reaction is carried out in an ice-water bath for 3 hours to obtain intermediate 1; Step 2, adding intermediate 1, triethylsilyl hydride and phosphonium cation solution into a container, reacting at 60° C. for 4 hours to obtain intermediate 2; Step 3, adding a sodium hydroxide solution and a dichloromethane solution of the intermediate 2 into a container, adding a dichloromethane solution of phosphorus oxychloride into the container, and reacting at room temperature for 2.5 hours to obtain the composite functional agent; The organic carrier is glycidylamine epoxy resin; The cross-linking agent is one of phthalic acid and terephthalic acid.
2. The conductive copper paste according to claim 1, characterized in that: The p-aminophenol solution in step 1 is prepared from 0.1 mol of p-aminophenol and 30-36 g of ethyl acetate, and the amount ratio of maleic anhydride, ethyl acetate, p-aminophenol solution, cyanuric chloride, tetrahydrofuran and triethylamine used is 0.1 mol: 220-240 g: 41-47 g: 18-20 g: 72-80 g: 24-30 g.
3. The conductive copper paste according to claim 1, characterized in that: The phosphonium cation solution in step 2 is prepared from 1 g of [(C6F5)3PF][B(C6F5)4] and 150-180 g of dichloromethane, and the usage ratio of intermediate 1, triethylsilyl hydride and phosphonium cation solution is 0.08 mol: 0.08-0.1 mol: 151-181 g.
4. The conductive copper paste according to claim 1, characterized in that: The sodium hydroxide solution in step 3 is prepared from 1.5g of sodium hydroxide and 5g of ultrapure water, the dichloromethane solution of intermediate 2 is prepared from 0.06mol of intermediate 2 and 40g of dichloromethane, and the dichloromethane solution of phosphorus oxychloride is prepared from 0.02mol of phosphorus oxychloride and 15g of dichloromethane. The amount ratio of the sodium hydroxide solution, the dichloromethane solution of intermediate 2, and the dichloromethane solution of phosphorus oxychloride is 6.5g:58.3g:18g.
5. A method for preparing a conductive copper slurry, characterized in that: The following steps are involved: Step 1: Weigh and screen each raw material according to mass fraction; Step 2: After the copper powder is acid-washed and ethanol-washed, it is stirred and mixed with the composite functional agent, and heat-treated to obtain the copper powder coated with the composite functional agent; Step 3: Fully mix the copper powder coated with the composite functional agent, nano silicon dioxide, an organic carrier, and a cross-linking agent to obtain the conductive copper slurry; The composite functional agent is prepared by the following steps: Step 1, maleic anhydride and ethyl acetate are added to a container, and the container is placed in an ice-water bath environment, and p-aminophenol solution is added to the container. After the addition is completed, the ice-water bath is removed, and the filtered product and cyanuric chloride, tetrahydrofuran, and triethylamine are added to the container, and the reaction is carried out in an ice-water bath for 3 hours to obtain intermediate 1; Step 2, adding intermediate 1, triethylsilyl hydride and phosphonium cation solution into a container, reacting at 60° C. for 4 hours to obtain intermediate 2; Step 3, adding a sodium hydroxide solution and a dichloromethane solution of the intermediate 2 into a container, adding a dichloromethane solution of phosphorus oxychloride into the container, and reacting at room temperature for 2.5 hours to obtain the composite functional agent; The organic carrier is glycidylamine epoxy resin; The cross-linking agent is one of phthalic acid and terephthalic acid.
6. The method for preparing a conductive copper paste according to claim 5, characterized in that: The particle size of the copper powder is 100nm-3μm.
7. The method for preparing a conductive copper paste according to claim 5, characterized in that: In the second step, the acid used for pickling is 15% by mass hydrochloric acid, the ethanol used for ethanol washing is 98% by mass industrial ethanol, the temperature condition of heat treatment is 55-65°C, and the time condition of heat treatment is 90-120min.
8. The method for preparing a conductive copper paste according to claim 5, characterized in that: The mixing temperature in the third step is 35-45°C and the mixing time is 30-45 min.
Citation Information
Patent Citations
Preparation method of silver coated copper powder for electronic slurry
CN102328076A
Medium temperature sintering copper-based conductive electronic paste
CN108231242A