A substrate for a flexible circuit board and a preparation method thereof, and a flexible circuit board

By setting up exhaust passages and low melting point resin on polyphenylene sulfide film or sheet, the problems of peeling off the substrate from copper foil and high energy consumption in copper clad plate are solved, and high dielectric of high frequency and high speed antennas are realized Performance and stable peel strength.

CN118612943BActive Publication Date: 2024-11-01四川力博为新材料有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410163095.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-11-01
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

During the preparation of copper clad plate, due to insufficient exhaust gas, the peeling force between the substrate and the copper foil is unstable, and bubble defects exist, and high-frequency and high-speed antennas have higher requirements on antenna quality. The existing polyphenylene sulfide materials are currently available. It is excellent in dielectric performance at high frequencies but high energy consumption in the bonding process, making it difficult to ensure high bridging strength.

Method used

ABA three-layer structure substrate is prepared using modified polyphenylene sulfide film or sheet, with exhaust passages on at least one side surface, through a granular matte surface or cross wedge-shaped groove twill structure, combined with the use of low melting point resin, to ensure the metal layer Close fit and efficient bonding to the substrate to avoid damage to the molecular chain structure.

Benefits of technology

It solves the defect of peeling off the substrate and copper foil, reduces the energy consumption of the bonding process, improves the bonding efficiency of the PPS film and copper foil, meets the requirements of high-frequency and high-speed antennas for dielectric and mechanical properties, and optimizes the The exhaust passage structure is enhanced to enhance the peel strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a substrate for a flexible circuit board, a preparation method thereof, and a flexible circuit board. The surface of at least one side of the substrate is set to a granular frosted surface, Ra is 0.5-5μm, Rz is 3-60μm, and an exhaust passage is formed between the particles; or the surface of at least one side of the substrate is set to a cross wedge groove twill, and the wedge grooves are connected to form an exhaust passage. The substrate prepared by the present invention can improve or avoid the defect of peeling between the substrate and the copper foil due to insufficient exhaust when preparing the copper clad laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a substrate for a flexible circuit board and a preparation method thereof, and a flexible circuit board. Background Art

[0002] With the popularization of 5G communications, the use of high-frequency and high-speed antennas in base station equipment has increased rapidly, and the quality requirements for antennas have become increasingly stringent. Polyphenylene sulfide materials are one of the best substrates for flexible copper clad laminates due to their excellent dielectric properties at high frequencies, low water absorption, high mechanical strength, high stiffness, high heat resistance, excellent corrosion resistance and outstanding flame retardancy. Summary of the invention

[0003] Research has found that due to poor exhaust, defects such as bubbles and unstable peeling force often occur at the joints between the PPS film and metal layers such as copper foil. In the first aspect, a substrate for a flexible circuit board is provided, which not only meets the requirements of mechanical properties and dielectric properties of high-frequency and high-speed copper-clad laminate substrates, but also solves the problem of the defect of the substrate and the copper foil peeling caused by insufficient exhaust when preparing the copper-clad laminate. The substrate is provided with an exhaust passage on at least one side surface for connection with the metal layer.

[0004] In one embodiment, at least one side of the substrate surface is set to a granular frosted surface, Ra is 0.5-5μm, Rz is 3-60μm, and an exhaust passage is formed between the particles; or at least one side of the substrate surface is set to a cross wedge groove twill, and the wedge grooves are connected to form an exhaust passage. The wedge groove twill is distributed at 45° along the longitudinal direction of the substrate, and the twills on both sides are arranged crosswise at 90°. The upper width of the wedge groove is 3-5μm, the bottom width (lower width) is 0.1-0.5μm, and the center interval between the twills is 3-60μm. If the copper clad laminate is double-layered, both sides are set to have exhaust passages to facilitate the subsequent preparation of the copper clad laminate.

[0005] The substrate is selected from modified polyphenylene sulfide film or sheet. The applicant selects an ABA three-layer structure. The melting point of the first PPS resin used in layer A is lower than the melting point of the second PPS resin used in layer B. The overall thickness is 25-1500 μm.

[0006] In one embodiment, an exhaust passage is arranged on the surface of the A layer, and the A layer is prepared by comprising the following components in parts by weight: 79-100 parts of a first PPS resin, 0-20 parts of a toughening and modifying resin, and 0.1-1 parts of an antioxidant.

[0007] In one embodiment, the melt index of the first PPS resin is selected from 100-600 g / 10 min.

[0008] The first PPS resin has a melting point lower than that of the second PPS resin, and preferably has a melt index of 200-500 g / 10 min, more preferably 300-400 g / 10 min.

[0009] Preferably, the toughening modified resin is used in an amount of 2-15 parts, more preferably 5-10 parts.

[0010] In one embodiment, the B layer is prepared by the following components in parts by weight: 39-100 parts of the second PPS resin, 0-60 parts of the inorganic filler, 0-20 parts of the toughening and modifying resin, and 0.1-1 parts of the antioxidant, and the component dosage is not zero. Preferably, the second PPS resin dosage is 42-80 parts, more preferably 50-65 parts; the inorganic filler dosage is 10-50 parts, more preferably 30-50 parts; the toughening and modifying resin dosage is 2-15 parts, more preferably 5-10 parts.

[0011] In one embodiment, the melt index of the second PPS resin is selected from 5-200 g / 10 min, preferably 10-150 g / 10 min, more preferably 20-100 g / 10 min.

[0012] In one embodiment, the inorganic filler is selected from one or a combination of two or more of silica, barium sulfate, talc, and ceramic powder whose surface is modified with alkoxysilane containing epoxy, amino or isocyanate groups; the particle size of the inorganic filler is 100nm-100μm, preferably 800nm-50μm, and more preferably 1μm-10μm; the toughening modified resin is one of polycarbonate, polyetherimide, polyethersulfone or polysulfone; the antioxidant is selected from one or a combination of two or more of antioxidant No. 1076, antioxidant 1010, antioxidant 168, and antioxidant 1035.

[0013] In the second aspect, a method for preparing a substrate for a flexible circuit board is provided, comprising the following contents: preparing a modified resin for the substrate, drying and removing water from the modified resin and adding it to a cast extrusion casting machine, and after melting and plasticizing, stretching, cooling, and shaping through three rollers to prepare the substrate, wherein the surface of the three rollers has a structure that forms an exhaust passage on the surface of the substrate.

[0014] In one embodiment, the temperature of the three rollers is selected from 10-200°C, preferably 20-150°C, and more preferably 40-140°C.

[0015] In a third aspect, a flexible circuit board is provided, which adopts the above-mentioned substrate for a flexible circuit board, and a metal layer is provided on at least one surface of the substrate.

[0016] The beneficial effects of the present invention are:

[0017] The substrate prepared by the present invention can improve or avoid the defect of peeling between the substrate and the copper foil due to insufficient exhaust when preparing the copper clad laminate. The surface layer uses a low melting point resin for low temperature bonding, which protects the molecular order of the middle layer from being destroyed, maintains the original performance of the PPS film layer, and can also reduce the energy consumption of the bonding process of the PPS film and the copper foil. In general, the anchoring effect is enhanced by making the surface of the copper foil concave and convex, but it cannot be guaranteed or is extremely difficult to ensure a high bridging strength with the surface of the substrate. With regard to this point, the surface treatment of the present invention meets the requirements of exhaust and high bridging strength by adopting an exhaust passage structure on the surface of the substrate. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0019] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0020] In the subsequent process of preparing flexible circuit boards, it was found that the molecular chain structure of the PPS film was easily damaged, and the material's high temperature resistance, stiffness and other properties would decrease accordingly.

[0021] The present invention provides a modified polyphenylene sulfide film or sheet, which is prepared into an ABA three-layer structure (thickness of 25μm-1500μm) by a three-layer co-extrusion casting device. The middle B layer of the film is a high-temperature resistant layer with orderly molecular chains, and the A layers on both sides are low-melting point layers with special exhaust textures. The PPS film produced by the casting method can make the molecular chains arranged in an orderly manner in the longitudinal stretching direction, giving a certain high-temperature resistance, wherein a large amount of fillers can also play a skeleton support role, giving the PPS film high stiffness and certain high-temperature resistance. In the subsequent process of preparing a flexible circuit board, the PPS film needs to be heated to a molten state before it can be closely fitted with the copper foil. Although it is still a PPS film after melting and cooling, the highly directional arrangement of the molecular chains has been destroyed, and its excellent high-temperature resistance, high stiffness and other characteristics can no longer be maintained. After a lot of research, the applicant has proposed a new solution. In the subsequent processing of the flexible circuit board, it is only necessary to melt the A layer resin to achieve bonding with the metal layer such as the copper foil. At this time, the B layer resin has not reached the melting point, the orderly molecular arrangement structure will not be destroyed, and the excellent function of the B layer is still maintained. The low melting point resin is melted with low energy consumption and short time, which improves the efficiency of the bonding process between PPS film and copper foil. At the same time, the special exhaust texture of the A layer also optimizes the defects such as bubbles between the substrate and the copper foil and unstable peeling force caused by poor exhaust.

[0022] The A layer contains a low melting point PPS resin, a toughening modified resin and an antioxidant. The surface of the A layer contains a special exhaust texture to form an exhaust passage. The B layer is a modified polyphenylene sulfide layer, which contains PPS resin, an inorganic filler, a toughening modified resin and an antioxidant.

[0023] Modified PPS resin used to prepare layer A and layer B:

[0024] Preparation of modified PPS resin for layer A: Dry the low-melting point first PPS resin at 90-140°C for 3-5h, mix the dried low-melting point first PPS resin with an appropriate amount of toughening modified resin and antioxidant in a high-speed mixer, add it into a twin-screw extruder to melt and plasticize and mix evenly (the processing temperature range of the twin-screw is 50-320°C), extrude, draw strips, and pelletize to prepare the low-melting point first modified PPS resin.

[0025] Preparation of modified PPS resin for layer B: Dry the second PPS resin at 130-150°C for 3-5h, mix the dried second PPS resin, inorganic filler, toughening modified resin and antioxidant in a high-speed mixer, add them into a twin-screw extruder for melt plasticization and mixing (processing temperature range is 50-350°C), extrude, draw strips, and pelletize to prepare the second modified PPS resin.

[0026] The products in Examples 1-8 were prepared as described above. The materials used to prepare the modified PPS resins for the A and B layers are as follows. The amounts of the components in the following contents are expressed in parts by weight:

[0027] Table 1 Composition and amount of the first modified PPS resin (layer A) (parts)

[0028]

[0029] Table 2 Composition and amount of the second modified PPS resin (layer B) (parts)

[0030]

[0031] The above examples provide the dosage of some components as an implementable solution of the present technology, and the specific contents are as follows:

[0032] First modified PPS resin (A layer):

[0033] The content of the first PPS resin is ≥ 79 parts, and its melting point is lower than that of the second PPS resin used in layer B, and its melt index is 100-600 g / 10min, preferably 200-500 g / 10min, and more preferably 300-400 g / 10min.

[0034] The content of the toughening and modifying resin is 0-20 parts, preferably 2-15 parts, more preferably 5-10 parts. The toughening and modifying resin can be polycarbonate, polyetherimide, polyethersulfone, or polysulfone.

[0035] The content of antioxidant is 0.1-1 part. This application provides an embodiment of 0.3 part dosage, and other dosages such as 0.2, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.7, 0.8, 0.9, etc. are all applicable. It can be one or a combination of two or more of the commercially available brands such as antioxidant 1076, antioxidant 1010, antioxidant 168, and antioxidant 1035. This application provides an example of using a combination of two antioxidants. In actual production, a single antioxidant or a combination of multiple antioxidants can be selected as needed.

[0036] Second modified PPS resin (layer B):

[0037] The second PPS resin content is 39-100 parts, preferably 42-80 parts, more preferably 50-65 parts. If the second PPS resin content is too low, the film or sheet is not easy to process. If the second PPS resin content is too high, the film or sheet has poor stiffness. The melt index is 5-200 g / 10min, preferably 10-150 g / 10min, more preferably 20-100 g / 10min.

[0038] The content of inorganic filler is 0-60 parts, preferably 10-50 parts, more preferably 30-50 parts. If the content of inorganic filler is too high, the film or sheet is not easy to process. If the content of inorganic filler is too low, the stiffness of the film or sheet is poor. The inorganic filler can be one or a combination of two or more of silicon dioxide, barium sulfate, talcum powder, ceramic powder, etc., which have been surface-modified with alkoxysilane containing epoxy, amino or isocyanate groups. Existing commercial products or any products disclosed in the prior art can be used. The particle size of the inorganic filler is 100nm-100μm, preferably 800nm-50μm, and more preferably 1μm-10μm. The above amount does not take a zero value, and an amount close to zero can be selected. The specific amount is determined according to the actual situation. The interpretation of zero values ​​in the following components is the same.

[0039] The toughening modified resin content is 0-20 parts, preferably 2-15 parts, more preferably 5-10 parts. If the toughening modified resin content is too low, the toughening effect of the film or sheet is not obvious. If the content is too high, the film or sheet has poor stiffness or high cost. The toughening modified resin can be one or a combination of two or more of polycarbonate, polyetherimide, polyether sulfone, and polysulfone. The toughening modified resin can be an existing commercial product or any product disclosed in the prior art.

[0040] The content of antioxidant is 0.1-1.0 parts. This application gives an example of 0.3 parts. Other amounts such as 0.2, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.7, 0.8, 0.9, etc. are all applicable. It can be one of the commercially available brands of antioxidant 1076, antioxidant 1010, antioxidant 168, antioxidant 1035, or a combination of two or more. This application gives an example of using a combination of two antioxidants. In actual production, a single antioxidant or a combination of two or more antioxidants can be selected according to needs.

[0041] Preparation of cast (or calendered) film or sheet:

[0042] After drying and removing water from the first modified PPS resin, add it to the hopper of the cast (or calender) extrusion casting machine 1#, melt and plasticize it, and extrude it from the A layers on both sides of the three-layer hanger die. After drying and removing water from the second modified PPS resin, add it to the hopper of the cast (or calender) extrusion casting machine 2#, melt and plasticize it, and extrude it from the middle B layer of the three-layer hanger die. After stretching, cooling and shaping by three rollers, it is prepared into a PPS sheet or film. The three rollers can be rubber rollers or steel rollers, and the roller surface is a granular frosted structure or a 90° cross-wedge groove twill. After the molten material is shaped and cooled by the rollers, the granular frosted structure or the 90° cross-wedge groove twill is printed on the surface of the A layer of the film or sheet. If the roller temperature is too low, the melt cools too quickly, and the thermal stress of the PPS resin cannot be fully released, resulting in excessive shrinkage of the film or sheet, which is easy to warp and deform in the subsequent copper clad laminate processing. If the roller temperature is too high, the roller will stick and cannot be produced smoothly. The temperature of the three rollers is about 10°C to about 200°C, preferably 20°C to about 150°C, and more preferably 40°C to about 140°C. The present invention provides a specific embodiment, which sequentially passes through a 50°C front roller, a 100°C middle roller, and a 130°C rear roller. The casting / calendering can also be performed at a temperature including but not limited to the following, which sequentially passes through a 50°C front roller, a 90°C middle roller, and a 120°C rear roller.

[0043] Table 3 Process and product performance of films or sheets for flexible circuit boards

[0044]

[0045] The texture of the surface of layer A is a granular frosted surface, with Ra of 0.5-5μm and Rz of 3-60μm. This application only provides some products with applicable Ra and Rz data. Other products are applicable as long as they meet the values ​​of Ra of 0.5-5μm and Rz of 3-60μm. The contours between particles are independent and distinct, and the contour valleys are interconnected to form channels for air evacuation. This is conducive to the vacuum extraction of air from the interconnected contour valleys during the subsequent copper clad laminate processing.

[0046] The surface texture of layer A can also be a 90° crossed wedge groove twill. The wedge groove twill is distributed at 45° along the longitudinal direction of the film or sheet, and the twills on both sides are arranged at 90°. This application only provides some applicable products with upper width, lower width, and spacing data. Other products are applicable as long as they meet the wedge groove upper width of 3-5μm, bottom width (lower width) of 0.1-0.5μm, and the center spacing between the twills is 3-60μm. The purpose of vacuum extraction of air from the interconnected wedge groove channels is achieved.

[0047] The present application provides a method for preparing a flexible circuit board, which uses a hot rolling process to cover copper foil on both sides of a substrate, and forms a flexible copper-clad laminate after lamination.

[0048] In this step, the press used in the hot rolling process can be a hydraulic high-temperature press manufactured by LAUFFER of Germany, model RMV2100. By using high-temperature heat-conducting oil, the oil pressure temperature of the vacuum high-temperature press can reach up to 400°C and be stable. The pressing temperature and pressure are determined by referring to the properties of layer A. For example, the parameters can be selected as follows: the maximum temperature does not exceed 220°C; the heating rate is recommended to be 4°C to 10°C / min; keep warm at 180 to 220°C for 1 to 2 hours; then cool down to room temperature, and the cooling rate should not exceed the heating rate.

[0049] That is to say, after the modified PPS sheet is extruded by the extruder, the sheet and the prepared copper foil with adhesive are immediately connected to the high-temperature press for calendering to obtain the copper-clad laminate. The high-temperature press can use metal rollers or silicone rubber rollers, and the recommended temperature is 180℃~220℃. The roller gap is set according to the thickness requirements of the copper-clad laminate.

[0050] Including but not limited to the contents disclosed in the preparation method, other processes may also be used for preparation. The present application takes the preparation of double-layer copper clad laminates as an example, but is not limited to double-layer copper clad laminates, and single-layer copper clad laminates are also applicable.

[0051] The surface-treated copper foil constituting the present invention can be manufactured by any method. Therefore, the copper foil can be an electrolytic copper foil, a rolled copper foil, a reverse copper foil, and a low-profile electrolytic copper foil, and the thickness can be selected from 18um, 35um, or 70um. In addition, the copper foil is preferably a non-roughened copper foil, but as long as it does not hinder the formation of the wiring pattern during the manufacture of the printed circuit board, it can also be a copper foil that has been roughened twice by pre-roughening, soft etching, cleaning, and oxidation-reduction treatment. There is no particular limitation on the thickness of the copper foil, which can be determined according to actual conditions or from existing commercial products or the methods disclosed in the prior art, and can be used as a reference.

[0052] As described above, the copper foil of the present invention can also be provided in the form of a copper foil with a carrier. In the case of an extremely thin copper foil, handling properties can be improved by making it into a copper foil with a carrier. The copper foil with a carrier can adopt a known layer structure without particular limitation.

[0053] In addition to copper foil, the metal layer can also be nickel foil, stainless steel foil, aluminum foil and other metal foils.

[0054] The film or sheet prepared by the above process was used to prepare a copper-clad product, and the schemes of Examples 5 and 6 were adopted to replace the three casting rollers with smooth surfaces to obtain a comparative copper-clad product, and the peel strength was tested according to GB / T 4722-2017. The performance data are as follows:

[0055] Table 4 Peel strength of copper-clad products prepared by different processes

[0056]

[0057] It can be seen from Table 4 that, compared with the substrate without an exhaust passage, the substrate for a flexible circuit board with an exhaust passage prepared by the present invention has better peel strength when made into a copper-clad product. In addition, by adjusting the size and shape of the exhaust passage, the peel strength of the copper-clad product also changes accordingly. The substrate for a flexible circuit board and its preparation method, and the flexible circuit board provided by the present invention meet the requirements of product exhaust and high bridging strength, while maintaining the original performance of the PPS film layer, it can also reduce the energy consumption of the PPS film and copper foil bonding process, and has good application prospects.

[0058] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A substrate for a flexible circuit board, characterized in that: The surface of at least one side of the substrate is provided with an exhaust passage for connecting with the metal layer; the surface of at least one side of the substrate is set to a granular frosted surface with Ra of 0.5-5μm and Rz of 3-60μm, and an exhaust passage is formed between the particles. The substrate is selected from a modified polyphenylene sulfide film or sheet, and an ABA three-layer structure is selected, and the melting point of the first PPS resin used in the A layer is lower than the melting point of the second PPS resin used in the B layer; or the surface of at least one side of the substrate is set to a cross wedge-shaped groove twill, and the wedge-shaped grooves are connected to form an exhaust passage; the wedge-shaped groove twill is distributed at 45° along the longitudinal direction of the substrate, and the twills on both sides are cross-arranged at 90°, the upper width of the wedge-shaped groove is 3-5μm, the bottom width is 0.1-0.5μm, and the center interval between the twills is 3-60μm.

2. The flexible circuit board substrate according to claim 1, characterized in that: The substrate is selected from modified polyphenylene sulfide film or sheet, and is configured with an ABA three-layer structure, wherein the melting point of the first PPS resin used in the A layer is lower than the melting point of the second PPS resin used in the B layer; the exhaust passage is arranged on the surface of the A layer, and the A layer is prepared by comprising the following components in parts by weight: 79-100 parts of the first PPS resin, 0-20 parts of the toughening modified resin, and 0.1-1 parts of the antioxidant; The B layer is prepared by including the following components in parts by weight: 39-100 parts of a second PPS resin, 0-60 parts of an inorganic filler, 0-20 parts of a toughening and modifying resin, and 0.1-1.0 parts of an antioxidant, and the amounts of the components are not zero.

3. The flexible circuit board substrate according to claim 2, characterized in that: The melt index of the first PPS resin is selected from 100-600 g / 10 min.

4. The flexible circuit board substrate according to claim 2, characterized in that: The melt index of the second PPS resin is selected from 5-200 g / 10 min.

5. The flexible circuit board substrate according to any one of claims 2 to 4, characterized in that: The inorganic filler is selected from one or a combination of two or more of silica, barium sulfate, talc, and ceramic powder whose surface is modified with alkoxysilane containing epoxy, amino or isocyanate groups; the toughening modified resin is polycarbonate, polyetherimide, polyethersulfone or polysulfone; the antioxidant is selected from one or a combination of two or more of antioxidant No. 1076, antioxidant 1010, antioxidant 168, and antioxidant 1035.

6. A method for preparing a substrate for a flexible circuit board, characterized in that: The present invention comprises the following contents: preparing a modified resin for use as a substrate for a flexible circuit board as described in any one of claims 2-5, drying and removing water from the modified resin, and then adding the modified resin into a cast extrusion sheet casting machine, and after melting and plasticizing, stretching, cooling, and shaping through three rollers to prepare the substrate, wherein the surface of the three rollers has a structure that forms an exhaust passage on the surface of the substrate.

7. The method for preparing a substrate for a flexible circuit board according to claim 6, characterized in that: The temperature of the three rollers is selected from 10-200°C.

8. A flexible circuit board, wherein a metal layer is provided on at least one surface of the flexible circuit board substrate according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Wearproof high temperature resistant flame retardant film or sheet and preparation method thereof

    CN106633771A

  • A multilayer circuit board and its manufacture method

    CN1964602A

  • Copper foil for printed circuit and copper foil with resin adhesive for printed circuit and copper-clad lamination board for printed circuit using it

    JP1998341066A

  • Method for manufacturing printed-wiring board

    JP2001358463A

  • Manufacturing method of wiring board

    JP2005072455A