A method for demulsification and coagulation of perfluoroether elastomer emulsion and a low-temperature demulsification system
Through the low-temperature demulsification system, the low-temperature freezing technology of liquid nitrogen or liquid carbon dioxide is used to solve the problems of agglomeration and metal ion pollution of perfluoroether elastomer emulsion, achieving the preparation of powder with uniform particle size and simplifying the subsequent treatment process.
Patent Information
- Application Number
- CN202411081988.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The existing chemical demulsification and coagulation methods for perfluoroelastic emulsions require the addition of inorganic electrolyte coagulation agents, resulting in rapid agglomeration, difficult to clean encapsulation impurities, uneven particle size, and easy residual metal ions to contaminate the semiconductor process.
Using a low-temperature demulsification system, the perfluoroelastomer concentrate is obtained by centrifugation and sprayed into the low-temperature inert liquid liquid in the form of liquid droplets for demulsification and condensation, and the polymer chain segments are frozen using low-temperature nitrogen or liquid carbon dioxide. Avoid agglomeration and impurity residues to achieve powder preparation with uniform particle size.
Rapid frozen demulsification of perfluoroelastomers is achieved, avoiding particle agglomeration and agglomeration, simplifying the subsequent processing process, such as devolatilization and end group passivation, and reducing the risk of metal ion contamination.
Smart Images

Figure CN118620106B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of perfluoroether elastomer synthesis, and in particular to a method for demulsification and coagulation of a perfluoroether elastomer emulsion and a low-temperature demulsification system. Background Art
[0002] When perfluoroether elastomers are synthesized by emulsion polymerization, the first thing obtained is an emulsion containing perfluoroether elastomers. After degassing, the solid content of the emulsion is usually 20-35%, and the particle size of the perfluoroether elastomer in the emulsion ranges from 0.1 to 1μm. The composition of the emulsion is complex, mainly including: perfluoroether elastomers polymerized from monomers, emulsifiers, initiators, stabilizers, pH buffers, chain transfer agents, small molecule polymers and water. The separation of perfluoroether elastomers and other components in the emulsion is the demulsification and coagulation process. There are many ways of demulsification and coagulation, which can generally be divided into two types: chemical demulsification and coagulation (electrolyte method, demulsifier method, etc.) and physical demulsification and coagulation (high-speed centrifugation method, electrostatic demulsification method, heating method, etc.).
[0003] Chemical demulsification requires the addition of flocculants. Existing flocculants mainly include inorganic salts such as magnesium chloride and inorganic acids such as dilute nitric acid. The main problem of using flocculants for flocculation is that the flocculation process quickly agglomerates, and the impurities are not easy to clean. At the same time, the large agglomerated particles are not conducive to subsequent treatment processes, such as devolatilization and end group passivation. When the particles are large, diffusion in processes such as devolatilization and end group passivation is a controlling step. When the particles are too small or the particle distribution range is large, the bed pressure drop in the fixed bed is large and channeling is easy to occur. Therefore, regulating the size and uniformity of the particles during the coagulation process is an indispensable step. In addition, the chemical demulsification method is prone to residual metal ions during the flocculation process. The residual metal ions are easy to release metal ions during semiconductor processes such as etching and photolithography, resulting in pollution to the semiconductor process.
[0004] Based on this, the present invention provides a new technical solution. Summary of the invention
[0005] In view of this, the embodiments of this specification provide a method for demulsification and coagulation of a perfluoroether elastomer emulsion and a low-temperature demulsification system, without the need to add an inorganic electrolyte coagulant.
[0006] The embodiments of this specification provide the following technical solution: a method for demulsification and coagulation of a perfluoroether elastomer emulsion, comprising:
[0007] S1, centrifuging the perfluoroether elastomer emulsion to obtain a perfluoroether elastomer concentrated liquid and a residual liquid;
[0008] S2, spraying the concentrated perfluoroether elastomer liquid to disperse the concentrated perfluoroether elastomer liquid in the form of droplets into a low-temperature inert liquid for demulsification and aggregation, wherein the temperature of the low-temperature inert liquid is lower than the glass transition temperature of the perfluoroether elastomer;
[0009] S3, separating the demulsified coagulants in S2, dispersing and washing them in water, and filtering to obtain a filter cake;
[0010] S4. Dry the filter cake in vacuum to obtain perfluoroether elastomer powder.
[0011] Optionally, the centrifugal factor ω in step S1 2 R is 10000g~20000g.
[0012] Optionally, the spraying in step S2 is powered by compressed air, high-pressure nitrogen or high-pressure argon.
[0013] Optionally, the low-temperature inert liquid in step S2 is liquid nitrogen or liquid carbon dioxide.
[0014] Optionally, in step S1, separation is performed using a centrifugal separator, and a paint cloth is provided on the inner wall of the centrifugal separator.
[0015] Optionally, in step S1, after the perfluoroether elastomer emulsion is centrifuged, it is further centrifuged and washed with water.
[0016] Optionally, the varnished cloth is hydrophilically modified tetrafluoroethylene, polypropylene or polyvinylidene fluoride.
[0017] Optionally, the surface of the varnished cloth has a plurality of holes or grooves.
[0018] The present application also provides a low-temperature demulsification system, which is used in any of the above-mentioned methods for demulsification and coagulation of perfluoroether elastomer emulsions, wherein the low-temperature demulsification system comprises a high-pressure gas storage tank, a concentrated emulsion storage tank, a concentrated emulsion temporary storage tank and a low-temperature liquid storage tank, and the high-pressure gas storage tank and the concentrated emulsion storage tank are both connected to the concentrated emulsion temporary storage tank through pipelines;
[0019] The concentrated emulsion storage tank stores a perfluoroether elastomer concentrate, the high-pressure gas storage tank stores one of high-pressure air, nitrogen or argon, the low-temperature liquid storage tank stores liquid nitrogen or liquid carbon dioxide, and the concentrated emulsion temporary storage tank sprays the perfluoroether elastomer concentrate into the low-temperature liquid storage tank through a nozzle.
[0020] Optionally, the high-pressure gas storage tank is connected to a high-pressure gas cylinder, the high-pressure gas cylinder and the high-pressure gas storage tank are controlled by a valve, the high-pressure gas storage tank and the concentrated emulsion temporary storage tank are controlled by a valve, the concentrated emulsion storage tank and the concentrated emulsion temporary storage tank are controlled by a valve, and the concentrated emulsion temporary storage tank and the nozzle are controlled by a valve.
[0021] Compared with the prior art, the at least one technical solution adopted in the embodiments of this specification can achieve the following beneficial effects:
[0022] The technical solution of the present application concentrates the perfluoroether elastomer emulsion by centrifugation, and then mixes the perfluoroether elastomer concentrate with a low-temperature inert liquid. The perfluoroether elastomer concentrate is quickly cooled to reduce the perfluoroether elastomer in the emulsion to below the glass transition temperature, freeze the movement of the polymer chain segments, and destroy the stable double-charge structure of the emulsion, so that the emulsion is demulsified in a short time. Centrifugal concentration can avoid the unfavorable phenomenon of fluffy particles after demulsification due to high water content and low perfluoroether elastomer content in the emulsion, which is convenient for subsequent devolatilization and end group passivation treatment of the perfluoroether elastomer.
[0023] In addition, high-speed spraying allows the perfluoroether elastomer concentrate to fully contact the cryogenic liquid in the form of droplets, rapidly cool and freeze, and avoid agglomeration of the perfluoroether elastomer particles, thereby obtaining particles with uniform particle size, which is beneficial to subsequent processing processes such as washing, freeze-vacuum drying, devolatilization, and end group passivation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, they can also refer to these attached process schematic diagrams without paying any creative work.
[0025] Figure 1 It is a schematic diagram of the process of a method for demulsification and coagulation of a perfluoroether elastomer emulsion in the present application.
[0026] Figure 2 It is a schematic diagram of a low-temperature demulsification system of the present application.
[0027] In the figure: 1. High-pressure gas storage tank; 2. Concentrated emulsion storage tank; 3. Concentrated emulsion temporary storage tank; 4. Cryogenic liquid storage tank; 5. High-pressure gas cylinder; 6. Nozzle. DETAILED DESCRIPTION
[0028] The embodiments of the present application are described in detail below with reference to the accompanying drawings.
[0029] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.
[0030] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structures and / or functions described herein are merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. In addition, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, those skilled in the art will understand that it can be practiced without these specific details.
[0031] Chemical demulsification requires the addition of flocculants. Existing flocculants mainly include inorganic salts such as magnesium chloride and inorganic acids such as dilute nitric acid. The main problem with flocculation using flocculants is that agglomeration occurs quickly during the flocculation process, and the impurities are not easy to clean. At the same time, the large agglomerated particles are not conducive to subsequent treatment processes, such as drying, devolatilization and end group passivation treatment.
[0032] By adopting the rapid cooling technology, the emulsion is atomized and mixed with the low-temperature liquid at high speed in the form of droplets. The perfluoroether elastomer in the emulsion is quickly reduced to below the glass transition temperature, the movement of the polymer chain segments is frozen, and the emulsion breaks and coagulates in a short time.
[0033] The centrifugal concentrated emulsion can greatly improve the production efficiency of freezing and demulsification.
[0034] The centrifugal concentration and low temperature demulsification method can quickly and effectively achieve the concentration and demulsification of the emulsion. Centrifugal concentration is mainly based on the different densities between the target product perfluoroether elastomer and the aqueous solution, and uses the strong centrifugal force generated during high-speed rotation to achieve separation. The stronger the centrifugal field, the better the concentration effect.
[0035] Based on this, the present specification proposes a method for demulsification and coagulation of a perfluoroether elastomer emulsion, comprising:
[0036] S1, centrifuging the perfluoroether elastomer emulsion to obtain a perfluoroether elastomer concentrated liquid and a residual liquid;
[0037] S2, spraying the concentrated perfluoroether elastomer liquid to disperse the concentrated perfluoroether elastomer liquid in the form of droplets into a low-temperature inert liquid for demulsification and aggregation, wherein the temperature of the low-temperature inert liquid is lower than the glass transition temperature of the perfluoroether elastomer;
[0038] S3, separating the demulsified coagulants in S2, dispersing and washing them in water, and filtering to obtain a filter cake;
[0039] S4. Dry the filter cake in vacuum to obtain perfluoroether elastomer powder.
[0040] The centrifugal factor ω²R in S1 is 10000g~20000g. A centrifugal separator is used for separation, and a varnished cloth is arranged on the inner wall of the centrifugal separator. The varnished cloth is hydrophilically modified tetrafluoroethylene, polypropylene or polyvinylidene fluoride. The perfluoroether elastomer emulsion is fed from the bottom of the centrifugal separator, and the centrifugal residual liquid is discharged from the top of the centrifugal separator. The centrifuged perfluoroether elastomer concentrated liquid is distributed on the surface of the varnished cloth. The direction of centrifugal separation is perpendicular to the flow direction of the residual liquid, which can realize continuous centrifugal separation and improve the centrifugal efficiency.
[0041] Hydrophilic varnished cloth can adhere to perfluoroether elastomer particles mixed with surfactants and concentrate the perfluoroether elastomer; when using hydrophobic varnished cloth, the perfluoroether elastomer emulsion is partially demulsified, but this demulsification is uncontrollable, which is manifested as a larger particle size after demulsification or the particles after demulsification stick together to form a film, which is not conducive to the subsequent spray demulsification at a low temperature stage, and is even more unfavorable for subsequent drying, devolatilization and end group passivation treatment. The holes or grooves on the surface of the hydrophilic varnished cloth can increase the interception effect of perfluoroether elastomer particles and reduce the loss of perfluoroether elastomer caused by the flow of the emulsion.
[0042] In step S2, one of compressed air, high-pressure nitrogen or high-pressure argon is used as the power for spraying, and the low-temperature inert liquid is liquid nitrogen or liquid carbon dioxide. The temperature of liquid nitrogen and liquid carbon dioxide is much lower than the glass transition temperature of the perfluoroether elastomer. The spraying method can make the perfluoroether elastomer concentrate fully dispersed in the form of droplets, quickly cool down to below its glass transition temperature, and quickly demulsify. At the same time, the impact cutting brought about by the spraying process can effectively destroy the double-charge structure of the micelles, thereby improving the demulsification effect.
[0043] In the step S1, the density of the perfluoroether elastomer emulsion is 1.21-1.23 g / ml, and the viscosity is 2.81-3.02 cp; the density of the concentrated emulsion is 1.27-1.31 g / ml, and the viscosity is 30000-35000 cp; the glass transition temperature of the perfluoroether elastomer is -10°C to -25°C.
[0044] In the technical solution of the present application, in order to avoid the introduction of impurities, unless otherwise specified, the water used is deionized water.
[0045] The method for determining the solid content in the perfluoroether elastomer emulsion is to take a certain mass of emulsion w1, dry it in an oven at 120°C for 24 h to obtain a solid, and weigh it after cooling, the mass is w2, the solid content is φ,
[0046] φ=w2 / w1×100%.
[0047] The solid obtained by drying includes perfluoroether elastomer polymerized from monomers, emulsifier, initiator, stabilizer, pH buffer, chain transfer agent, small molecule polymer and bound water.
[0048] The centrifugal separation and concentration process mainly removes water, and at the same time removes some free surfactants, initiators, pH buffers, chain transfer agents, small molecule polymers, etc.
[0049] The present application also provides a low-temperature demulsification system for implementing the above method, comprising a high-pressure gas storage tank 1, a concentrated emulsion storage tank 2, a concentrated emulsion temporary storage tank 3 and a low-temperature liquid storage tank 4, wherein the high-pressure gas storage tank 1 and the concentrated emulsion storage tank 2 are both connected to the concentrated emulsion temporary storage tank 3 through a pipeline.
[0050] The concentrated emulsion storage tank 2 stores perfluoroether elastomer concentrate, the high-pressure gas storage tank 1 stores one of high-pressure air, nitrogen or argon, the low-temperature liquid storage tank 4 stores liquid nitrogen or liquid carbon dioxide, and the concentrated emulsion temporary storage tank 3 sprays and disperses the perfluoroether elastomer concentrate into the low-temperature liquid storage tank through the nozzle 6.
[0051] The high-pressure gas storage tank 1 is connected to the high-pressure gas cylinder 5, the high-pressure gas cylinder 5 and the high-pressure gas storage tank 1 are controlled by a valve, the high-pressure gas storage tank 1 and the concentrated emulsion temporary storage tank 3 are controlled by a valve, the concentrated emulsion storage tank 2 and the concentrated emulsion temporary storage tank 3 are controlled by a valve, and the concentrated emulsion temporary storage tank 3 and the nozzle 6 are controlled by a valve.
[0052] Example 1
[0053] A method for demulsifying and coagulating a perfluoroether elastomer emulsion, comprising:
[0054] S1. Centrifuge 2500 mL (density 1.22 g / ml) of perfluoroether elastomer emulsion with a solid content of 31.6% with a centrifugal factor ω²R of 13500g. After centrifugation, use 2000 ml of water to recover the raw materials retained in the container and pipeline to obtain a perfluoroether elastomer concentrate v1 = 1027 mL (density 1.29 g / ml, viscosity 32000 cp) and a residual liquid v2 = 3350 mL; the inner wall of the centrifuge is provided with a hydrophilic 10-mesh PTFE varnish cloth (pore size 1.7 mm), and the residual liquid is flocculated and stirred with a 10% MgCl2 flocculant to precipitate a product. After drying, the precipitated product has a mass of 6.2g;
[0055] S2, spray v3 = 100 mL of the perfluoroether elastomer concentrate into an open liquid nitrogen (0.5 L, -195 ° C) using 4.5 bar nitrogen gas to break the emulsion and coagulate;
[0056] S3, after the liquid nitrogen evaporates, dispersing and washing the perfluoroether elastomer particles in S2 in water, and filtering to obtain a filter cake;
[0057] S4. The filter cake is vacuum dried to obtain 62.7 g of perfluoroether elastomer powder w3. The particle size of the powder is less than 1.0 mm (passing through a 16-mesh sieve). The glass transition temperature of the perfluoroether elastomer powder is -16.2 °C.
[0058] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and no product was precipitated, indicating that the demulsification and coagulation were complete.
[0059] Example 2
[0060] A method for demulsifying and coagulating a perfluoroether elastomer emulsion, comprising:
[0061] S1. Centrifuge 2500 mL (density 1.22 g / ml) of perfluoroether elastomer emulsion with a solid content of 31.6% with a centrifugal factor ω²R of 17500g. After centrifugation, use 2000 ml of water to recover the raw materials retained in the container and pipeline to obtain 982 mL of perfluoroether elastomer concentrate (density 1.30 g / ml, viscosity 34000 cp) and 3472 mL of residual liquid; the inner wall of the centrifuge is provided with a hydrophilic 10-mesh PTFE varnish cloth (pore size 1.7 mm), and the residual liquid is flocculated and stirred with a 10% MgCl2 flocculant to precipitate a product. After drying, the precipitated product has a mass of 7.4g.
[0062] S2. Spray 100 mL of the perfluoroether elastomer concentrate into an open liquid nitrogen (0.5 L, -195°C) using 4.5 bar nitrogen gas to break the emulsion;
[0063] S3, after the liquid nitrogen evaporates, dispersing and washing the perfluoroether elastomer particles in S2 in water, and filtering to obtain a filter cake;
[0064] S4. The filter cake is vacuum dried to obtain 67.4 g of perfluoroether elastomer powder w3. The particle size of the powder is less than 1.0 mm (passing through a 16-mesh sieve). The glass transition temperature of the perfluoroether elastomer powder is -15.9 °C.
[0065] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and no product was precipitated, indicating that the demulsification and coagulation were complete.
[0066] Example 3
[0067] The difference between the present embodiment and embodiment 1 is that the concentrated liquid obtained in step S1 is sprayed into sealed liquid carbon dioxide (0.5 L, saturated pressure and saturated temperature are 4.5 bar and -56°C, respectively) using 5.5 bar nitrogen to break the emulsion;
[0068] S3, releasing the pressure, dispersing and washing the perfluoroether elastomer particles in step S2 in water, and filtering to obtain a filter cake;
[0069] S4. The filter cake was vacuum dried to obtain 64.3 g of perfluoroether elastomer powder. The particle size of the powder was less than 1.0 mm (passing through a 16-mesh sieve). The glass transition temperature of the perfluoroether elastomer powder was -16.1 °C.
[0070] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and no product was precipitated, indicating that the demulsification and coagulation were complete.
[0071] Example 4
[0072] The difference between the present embodiment and embodiment 2 is that the concentrated liquid obtained in step S1 is sprayed into sealed liquid carbon dioxide (0.5 L, saturated pressure and saturated temperature are 4.5 bar and -56°C, respectively) using 5.5 bar nitrogen to break the emulsion;
[0073] S3, releasing the pressure, dispersing and washing the perfluoroether elastomer particles in S2 in water, and filtering to obtain a filter cake;
[0074] S4. The filter cake was vacuum dried to obtain 67.5 g of perfluoroether elastomer powder. The particle size of the powder was less than 1.0 mm (passing through a 16-mesh sieve). The glass transition temperature of the perfluoroether elastomer powder was -16.6 °C.
[0075] The filtrate in S3 was flocculated and stirred with 10% MgCl2 flocculant, and no product was precipitated, indicating that the demulsification and coagulation were complete.
[0076] Comparative Example 1
[0077] The difference between the embodiment of the present application and embodiment 1 is that the concentrated liquid obtained in step S2 is directly mixed with liquid nitrogen without spraying.
[0078] After demulsification, the perfluoroether elastomer aggregates into lumps, which makes it difficult to wash and carry out subsequent treatment processes such as devolatilization.
[0079] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and no product was precipitated, indicating that the demulsification and coagulation were complete.
[0080] Comparative Example 2
[0081] The difference between the embodiment of the present application and embodiment 1 is that the surface of the varnished cloth is hydrophobically modified tetrafluoroethylene.
[0082] Part of the concentrated emulsion obtained is directly demulsified to form membrane sheets, which are difficult to wash and cannot be post-processed by devolatilization and end group passivation.
[0083] No subsequent low-temperature emulsification was performed.
[0084] Comparative Example 3
[0085] The difference between the comparative example of the present application and Example 1 is that in step S2, the concentrated liquid is directly sprayed and mixed with anhydrous ethanol at room temperature.
[0086] Viscous inclusions are formed, which are difficult to wash and cannot be post-processed by devolatilization and end group passivation.
[0087] In step S4, the filter cake is vacuum dried to obtain 20 g of perfluoroether elastomer powder w3.
[0088] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and a large amount of product was precipitated. After the precipitated product was dried, the mass was 46.8 g, indicating that the demulsification and coagulation using anhydrous ethanol was incomplete.
[0089] Comparative Example 4
[0090] The difference between the embodiment of the present application and embodiment 1 is that in step S2, the concentrated liquid is directly sprayed with 80° C. hot water for dispersion and washing.
[0091] In step S4, the filter cake is vacuum dried to obtain 6.6 g of perfluoroether elastomer powder w3, with only a small amount of demulsification and aggregation.
[0092] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and a large amount of product was precipitated. After the precipitated product was dried, the mass was 59.8 g, indicating that the demulsification and coagulation using hot water were incomplete.
[0093] Comparative Example 5
[0094] The difference between the embodiment of the present application and embodiment 1 is that in step S2, the concentrated liquid is directly sprayed into a 0°C ice-water mixture, that is, a low-temperature liquid dispersion experiment is performed above the glass transition temperature of the perfluoroether elastomer.
[0095] In step S4, the filter cake is vacuum dried to obtain 13.4 g of perfluoroether elastomer powder w3, with only a small amount of demulsification and aggregation.
[0096] In step S3, the filtrate was flocculated and stirred with 10% MgCl2 flocculant, and a large amount of product was precipitated. After the precipitated product was dried, the mass was 53.7 g, indicating that the demulsification and coagulation using 0°C low-temperature water were incomplete.
[0097] Comparative Example 6
[0098] The difference between this comparative example and Example 1 is that the perfluoroether elastomer emulsion in step S1 is not concentrated by centrifugation, but 100 mL of the emulsion is directly sprayed into open low-temperature liquid nitrogen (0.5 L, -195°C).
[0099] Compared with the centrifugal concentration process, the filter cake obtained in this process is a fluffy body;
[0100] The filter cake was vacuum dried to obtain 27.5 g of perfluoroether elastomer powder. The powders were bridged and entangled and were not easy to pass through a sieve (80 mesh sieve).
[0101] 10% MgCl2 flocculant was added to S3 water and stirred. No product was precipitated, indicating that the demulsification and coagulation were complete.
[0102] Assume that the volume of the perfluoroether elastomer concentrated solution is v1, the volume of the residual solution is v2, the volume of the perfluoroether elastomer concentrated solution that is frozen and demulsified in step S2 is v3, the mass of the perfluoroether elastomer powder obtained after vacuum drying the filter cake is w3, and the mass of the product obtained by using 10% MgCl2 flocculant in the residual solution in step S1 is w4 (dry weight). Then the product recovery rate of the centrifugal concentration process is η1.
[0103] ,
[0104] Assuming that in step S3, the mass of the product obtained by using 10% MgCl2 flocculant in the filtrate is w5 (dry weight), the demulsification rate of using centrifugal concentration and low-temperature demulsification is η2,
[0105] η2=w3 / (w3+w5)
[0106] Table 1 shows the centrifugal concentration and low-temperature demulsification parameters, recovery rate and demulsification rate.
[0107]
[0108] By comparing Comparative Example 1 with Example 1, it can be seen that although the perfluoroether elastomer can be demulsified by direct mixing, the particles agglomerate due to direct mixing of the concentrated liquid, making it impossible to carry out subsequent treatment processes such as devolatilization.
[0109] By comparing Comparative Example 2 with Example 1, it can be seen that the use of hydrophobically modified tetrafluoroethylene as the paint cloth causes the perfluoroether elastomer to directly spread and adhere to the hydrophobic paint cloth, resulting in demulsification and agglomeration, and finally forming a membrane, which makes it impossible to perform subsequent low-temperature demulsification treatment, let alone subsequent devolatilization treatment.
[0110] By comparing Comparative Examples 3, 4, 5 with Example 1, it can be seen that when dispersing above the glass transition temperature, only a small amount of demulsification can be achieved, and the demulsification is incomplete and the efficiency is low.
[0111] By comparing Comparative Example 6 with Example 1, it can be seen that when the perfluoroether elastomer emulsion is directly subjected to low-temperature demulsification, due to the presence of a large amount of water in the perfluoroether elastomer emulsion, the obtained filter cake is relatively fluffy, and bridging and entanglement phenomena are easily generated between the particles, resulting in the perfluoroether elastomer powder being difficult to sieve, having low strength, and being unable to perform subsequent devolatilization and other treatment steps in the packed bed.
[0112] In this specification, the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments described later, the description is relatively simple, and the relevant parts can be referred to the partial description of the previous embodiments.
[0113] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for demulsification and coagulation of a perfluoroether elastomer emulsion, Features: S1, centrifugally separating the perfluoroether elastomer emulsion to obtain a perfluoroether elastomer concentrate and a residual liquid, and separating them by using a centrifugal separator, wherein a varnished cloth is arranged on the inner wall of the centrifugal separator, and the varnished cloth is made of hydrophilically modified tetrafluoroethylene, polypropylene or polyvinylidene fluoride; S2, spraying the concentrated perfluoroether elastomer liquid to disperse the concentrated perfluoroether elastomer liquid in the form of droplets into a low-temperature inert liquid for demulsification and aggregation, wherein the temperature of the low-temperature inert liquid is lower than the glass transition temperature of the perfluoroether elastomer; S3, separating the demulsified coagulants in S2, dispersing and washing them in water, and filtering to obtain a filter cake; S4. Dry the filter cake in vacuum to obtain perfluoroether elastomer powder.
2. A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to claim 1, Features: Centrifugal factor in step S1 / g is 10000~20000.
3. A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to claim 1, Features: In step S2, the injection is powered by compressed air, high-pressure nitrogen or high-pressure argon.
4. A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to claim 1, Features: In step S2, the low-temperature inert liquid is liquid nitrogen or liquid carbon dioxide.
5. A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to claim 1, Features: In step S1, after the perfluoroether elastomer emulsion is centrifuged, it is further centrifuged and washed with water.
6. A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to claim 1, Features: The surface of the varnished cloth is provided with a plurality of holes or grooves.
7. A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to claim 1, Features: The perfluoroether elastomer emulsion is fed from the bottom of the centrifugal separator, the centrifugal residual liquid is discharged from the top of the centrifugal separator, and the centrifugally separated perfluoroether elastomer concentrated liquid is distributed on the surface of the varnished cloth.
8. A low temperature demulsification system, Features: A method for demulsification and coagulation of a perfluoroether elastomer emulsion according to any one of claims 1 to 7, wherein the low-temperature demulsification system comprises a high-pressure gas storage tank, a concentrated emulsion storage tank, a concentrated emulsion temporary storage tank and a low-temperature liquid storage tank, and the high-pressure gas storage tank and the concentrated emulsion storage tank are both connected to the concentrated emulsion temporary storage tank through a pipeline; The concentrated emulsion storage tank stores a perfluoroether elastomer concentrate, the high-pressure gas storage tank stores one of high-pressure air, nitrogen or argon, the low-temperature liquid storage tank stores liquid nitrogen or liquid carbon dioxide, and the concentrated emulsion temporary storage tank sprays the perfluoroether elastomer concentrate into the low-temperature liquid storage tank through a nozzle.
9. The low-temperature demulsification system according to claim 8, It is characterized in that The high-pressure gas storage tank is connected to a high-pressure gas cylinder, the high-pressure gas cylinder and the high-pressure gas storage tank are controlled by a valve, the high-pressure gas storage tank and the concentrated emulsion temporary storage tank are controlled by a valve, the concentrated emulsion storage tank and the concentrated emulsion temporary storage tank are controlled by a valve, and the concentrated emulsion temporary storage tank and the nozzle are controlled by a valve.
Citation Information
Patent Citations
Recovery of polymer
JP1995233214A
Method for producing acrylic resin powder
JP2010235677A
Cryogenic processing methods and apparatus
US20030064141A1
Method for producing de-watered grafted rubber concentrate
US4857631A
Ultra-clean fluoropolymers
US6720360B1
Cited By
Preparation method of hydrophobic modified perfluoroether elastomer
CN121248828A
A process for the preparation of a hydrophobically modified perfluoroether elastomer
CN121248828B