A method for preparing anisotropic hydrogel with aniline-regulated polymer network structure

By adding aniline solvent to the polyvinyl alcohol solution and processing under specific temperature conditions, polyvinyl alcohol-based hydrogels with good flexibility and anisotropic structure are prepared, which solves the flexibility and flexibility of existing hydrogels. The lack of stretchability has achieved significant performance improvement in sensor applications.

CN118620240BActive Publication Date: 2024-11-29DEZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411052678.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-29
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The anisotropic hydrogels prepared by the existing ice template method are insufficient in terms of flexibility and stretchability, limiting their use in sensor applications, especially in cases such as patients at home or in exercise.

Method used

Polyvinyl alcohol-based hydrogels with anisotropic structures were prepared by dissolving polyvinyl alcohol using an aniline solvent, and cooling and thawing under specific temperature conditions.

Benefits of technology

The hydrogel prepared by this method has good flexibility and anisotropic structure. Compared with ordinary hydrogels, its strength, toughness, fatigue resistance and electrical conductivity have been significantly improved, and is suitable for flexible sensors and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118620240B_ABST
    Figure CN118620240B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing an anisotropic hydrogel of polymer network structure regulated by aniline, and the process is as follows: 18-20 mL of aniline solvent with a concentration of 0.04-0.05 mol / L is taken, polyvinyl alcohol (PVA) is dissolved at 93-97°C, and a polyvinyl alcohol solution with a concentration of 3-5 wt% is obtained; the solution is cooled to room temperature, and then cooled at -20°C for 24 hours and thawed at room temperature for 4 hours to obtain a polyvinyl alcohol-based aniline hydrogel. The polyvinyl alcohol-based hydrogel obtained by the method of the present invention has an anisotropic structure; compared with ordinary hydrogels, the hydrogel has more outstanding strength, toughness, fatigue resistance and conductivity, and has significant advantages in application in flexible sensors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wearable electronic devices, and in particular to a method for preparing an anisotropic hydrogel with a polymer network structure regulated by aniline. Background Art

[0002] The ice template method uses ice crystals as templates to prepare materials with microstructures and morphologies. In this process, the solvent, low temperature environment, cooling rate, etc. will affect the performance of the skeleton material, resulting in excessive reliance on external factors. The current ice template method mainly includes the preparation of magnetic Fe3O4 nanoparticles by solvothermal method, the modification of magnetic Fe3O4 nanoparticles to obtain magnetic Fe3O4 nanoparticles with unsaturated double bonds on the surface (Fe3O4-R), and then relying on the crosslinker, monomers AM (acrylamide) and AMPS (2-acrylamide-2-methylpropanesulfonic acid) and photoinitiator ketoglutaric acid to mix, and use ultraviolet radiation in a static magnetic field to prepare anisotropic AM / AMPS / Fe3O4-R hydrogel. The hydrogel prepared by the current method is a gel structure passively formed under external environmental conditions, resulting in its insufficient flexibility and stretchability. In particular, when the hydrogel is used on the sensor, it limits the detection of patients at home or in sports, and is easy to cause physical discomfort to the subject. Therefore, providing a hydrogel with good flexibility and anisotropy is of great significance in practical applications. Summary of the invention

[0003] In view of this, the present invention provides a method for preparing anisotropic hydrogels with aniline-regulated polymer network structures, specifically a method for preparing a polyvinyl alcohol solution by dissolving polyvinyl alcohol in an aniline solvent, cooling the polyvinyl alcohol solution at -20°C for 24 hours, and thawing it at room temperature for 4 hours to prepare a polyvinyl alcohol-based hydrogel. The hydrogel prepared by this method has good flexibility and anisotropy, and is suitable for use in sensors, cardiac tissue engineering and other fields.

[0004] The technical solution of the present invention is as follows:

[0005] A method for preparing an anisotropic hydrogel with aniline-regulated polymer network structure, the main process of which is as follows: taking 18-20 mL of aniline solvent with a concentration of 0.04-0.05 mol / L, dissolving polyvinyl alcohol (PVA) at 93-97°C to obtain a polyvinyl alcohol solution with a concentration of 3-5 wt%; cooling to room temperature, then cooling at -20°C for 24 hours and thawing at room temperature for 4 hours to obtain a polyvinyl alcohol-based aniline hydrogel;

[0006] In the present invention, aniline small molecules having a hydrophobic rigid benzene ring and a hydrophilic amino substituent will form hydrogen bonds and benzene ring π-π stacking effects with water molecules on the surface of ice crystals, inducing the water molecules to distribute in the optimal direction along the benzene ring in space, thereby achieving the purpose of actively regulating the microstructure of the hydrogel through molecular-level design, thereby enabling efficient, precise and controllable preparation of anisotropic hydrogels; the new method for preparing multi-scale anisotropic hydrogels proposed in the present invention is expected to achieve new breakthroughs in the synthesis and application of soft matter materials.

[0007] The polyvinyl alcohol-based hydrogel obtained by the method of the present invention has an anisotropic structure; compared with ordinary hydrogels, it has more outstanding strength, toughness, fatigue resistance and conductivity, and has significant advantages in application in flexible sensors.

[0008] Preferably, the aniline solvent is prepared by adding water to one of aniline (ANI), o-phenylenediamine (OPD), m-phenylenediamine (MPD) and p-phenylenediamine (PPD).

[0009] Preferably, 19 mL of aniline solvent with a concentration of 0.05 mol / L is mixed with 0.95 g of polyvinyl alcohol at 95° C. to obtain a PVA solution with a concentration of 4.75 wt %, and the pH of the PVA solution is 7.0±0.1.

[0010] Compared with the prior art, the beneficial effects of the present invention are:

[0011] 1. In the present invention, the small molecules of the aniline compounds having both aromatic rings and hydrophilic groups will form hydrogen bonds with the water molecules on the surface of the ice crystals and the dual effects of π-π stacking of the benzene rings, which determines the optimal distribution direction of the water molecules along the benzene rings in space, thereby achieving the purpose of actively regulating the growth direction of the ice crystals.

[0012] 2. In the present invention, by using aniline compounds, the purpose of actively regulating the microstructure of the hydrogel is achieved at the molecular level, and anisotropic hydrogels can be prepared efficiently, accurately and controllably.

[0013] 3. The new method for preparing multi-scale anisotropic hydrogel proposed in the present invention is expected to achieve new breakthroughs in the synthesis and application of soft matter materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0015] Figure 1These are SEM images of the hydrogels of Examples 1-5, where a is the SEM image of the PVA hydrogel; b is the SEM image of the PVA-ANI hydrogel; c is the SEM image of the PVA-OPD hydrogel; d is the SEM image of the PVA-MPD hydrogel; and e is the SEM image of the PVA-PPD hydrogel.

[0016] Figure 2 These are optical microscope images of the hydrogels of Examples 1-5, wherein a is an optical microscope image of a PVA hydrogel; b is an optical microscope image of a PVA-ANI hydrogel; c is an optical microscope image of a PVA-OPD hydrogel; d is an optical microscope image of a PVA-MPD hydrogel; e is an optical microscope image of a PVA-PPD hydrogel; and f is a schematic diagram of the orientation structure of the hydrogel.

[0017] Figure 3 FTIR graphs of the oriented PVA hydrogels mediated by Examples 1-5.

[0018] Figure 4 This is the XRD diagram of the hydrogel detected in Examples 1-5.

[0019] Figure 5 The figures are the test results of tensile and compressive properties of Examples 1-5, wherein a is the tensile stress-strain curve of PVA, PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels; b is the elastic modulus, toughness and maximum stress graph; c is the compressive stress-strain curve; d is the stretching cycle of PVA-OPD hydrogel under different strains.

[0020] Figure 6 These are the fatigue resistance test results of the hydrogels of Examples 1-5. In the figure, a is the first stretching loading and unloading curve of PVA, PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels at 150% strain; b is the energy dissipation and tensile stress change diagram of PVA, PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels; c is the stretching loading and unloading cycle curve of PVA-OPD hydrogel at 150% strain for 10 times; d is the energy dissipation and tensile stress change diagram of PVA-OPD hydrogel. DETAILED DESCRIPTION

[0021] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0022] Example 1

[0023] A method for preparing anisotropic hydrogel with aniline-regulated polymer network structure, the process is as follows:

[0024] (1) Preparation of aniline (ANI) solvent:

[0025] Take 0.23 mL of aniline and add 50 mL of water to prepare aniline solvent;

[0026] (2) Preparation of polyvinyl alcohol solution:

[0027] 19 mL of the aniline solvent prepared in step (1) was taken and mixed with 0.95 g of polyvinyl alcohol at 95° C. to obtain a PVA solution with a concentration of 4.75 wt %. The pH of the PVA solution was 7.0±0.1.

[0028] (3) Preparation of polyvinyl alcohol-based hydrogel:

[0029] The polyvinyl alcohol solution obtained in step (2) was cooled to room temperature, then cooled at -20°C for 24 hours and thawed at room temperature for 4 hours to obtain a PVA-ANI hydrogel.

[0030] Example 2

[0031] A method for preparing anisotropic hydrogel with aniline-regulated polymer network structure, the process is as follows:

[0032] (1) Preparation of o-phenylenediamine (OPD) solvent:

[0033] Take 0.27 mL of o-phenylenediamine and add 50 mL of water to prepare o-phenylenediamine solvent;

[0034] (2) Preparation of polyvinyl alcohol solution:

[0035] Take 19 mL of the o-phenylenediamine solvent prepared in step (1), mix it with 0.95 g of polyvinyl alcohol at 95° C. to obtain a PVA solution with a concentration of 4.75 wt %, and the pH of the PVA solution is 7.0±0.1;

[0036] (3) Preparation of polyvinyl alcohol-based hydrogel:

[0037] The polyvinyl alcohol solution obtained in step (2) was cooled to room temperature, then cooled at -20°C for 24 hours and thawed at room temperature for 4 hours to obtain a PVA-OPD hydrogel.

[0038] Example 3

[0039] A method for preparing anisotropic hydrogel with aniline-regulated polymer network structure, the process is as follows:

[0040] (1) Preparation of metaphenylenediamine (MPD) solvent:

[0041] Take 0.27 mL of m-phenylenediamine and add 50 mL of water to prepare m-phenylenediamine solvent;

[0042] (2) Preparation of polyvinyl alcohol solution:

[0043] 19 mL of the m-phenylenediamine solvent prepared in step (1) was taken and mixed with 0.95 g of polyvinyl alcohol at 95° C. to obtain a PVA solution with a concentration of 4.75 wt %, and the pH of the PVA solution was 7.0±0.1;

[0044] (3) Preparation of polyvinyl alcohol-based hydrogel:

[0045] The polyvinyl alcohol solution obtained in step (2) was cooled to room temperature, then cooled at -20°C for 24 hours and thawed at room temperature for 4 hours to obtain a PVA-MPD hydrogel.

[0046] Example 4

[0047] A method for preparing anisotropic hydrogel with aniline-regulated polymer network structure, the process is as follows:

[0048] (1) Preparation of p-phenylenediamine (PPD) solvent:

[0049] Take 0.27 mL of p-phenylenediamine and add 50 mL of water to prepare p-phenylenediamine solvent;

[0050] (2) Preparation of polyvinyl alcohol solution:

[0051] 19 mL of the p-phenylenediamine solvent prepared in step (1) was mixed with 0.95 g of polyvinyl alcohol at 95° C. to obtain a PVA solution with a concentration of 4.75 wt %, and the pH of the PVA solution was 7.0±0.1;

[0052] (3) Preparation of polyvinyl alcohol-based hydrogel:

[0053] The polyvinyl alcohol solution obtained in step (2) was cooled to room temperature, then cooled at -20°C for 24 hours and thawed at room temperature for 4 hours to obtain a PVA-PPD hydrogel.

[0054] Example 5

[0055] A method for preparing a hydrogel comprises the following steps: taking 19 mL of water, mixing it with 0.95 g of polyvinyl alcohol at 95° C. to obtain a PVA solution with a concentration of 4.75 wt %, wherein the pH value of the PVA solution is 7.0±0.1; cooling the polyvinyl alcohol solution to room temperature, then cooling it at -20° C. for 24 hours and thawing it at room temperature for 4 hours to obtain a PVA hydrogel.

[0056] Detection:

[0057] The hydrogels obtained in Examples 1-5 were tested, and the test items and results are as follows:

[0058] Figure 1 1-5 are SEM images of the hydrogels of Examples 1-5, wherein a is a SEM image of a PVA hydrogel; b is a SEM image of a PVA-ANI hydrogel; c is a SEM image of a PVA-OPD hydrogel; d is a SEM image of a PVA-MPD hydrogel; and e is a SEM image of a PVA-PPD hydrogel.

[0059] Figure 2 Figures are optical microscope images of the hydrogels of Examples 1-5, in which a is an optical microscope image of a PVA hydrogel; b is an optical microscope image of a PVA-ANI hydrogel; c is an optical microscope image of a PVA-OPD hydrogel; d is an optical microscope image of a PVA-MPD hydrogel; e is an optical microscope image of a PVA-PPD hydrogel; and f is a schematic diagram of the orientation structure of the hydrogel;

[0060] Combination Figure 1 and Figure 2 It can be seen that the microstructure of PVA hydrogel ( Figure 1 a) and ice crystal structure ( Figure 2 a) All of them are isotropic, while PVA-ANI hydrogel, PVA-OPD hydrogel, PVA-MPD hydrogel, and PVA-PPD hydrogel oriented by aniline derivatives show significant anisotropic structures. It can be seen that aniline derivatives play an important role in the directional growth and uniform distribution of ice crystals.

[0061] FTIR was used to detect the functional group structure of the hydrogel, and XRD was used to detect the crystallinity of the hydrogel. The results are shown in Figure 3 and Figure 4 ;

[0062] Figure 3 The FTIR images of hydrogels prepared with different aniline solvents are used to verify the intrinsic reasons why aniline compounds mediate the orientation of PVA hydrogels.

[0063] Combination Figure 3 It can be seen that in PVA hydrogel, 1090 cm -1 and 3380 cm -1 The characteristic peaks at 1090 cm -1 The characteristic peak shifted to 1100 cm -1The peak of -OH stretching vibration is red-shifted by 30 cm -1 , indicating that the amino groups in aniline compounds are conducive to forming hydrogen bonds with the hydroxyl groups of PVA, thereby enhancing the intermolecular interaction; the infrared spectrum of the hydrogel introduced with aniline compounds is at 1240 cm -1 The NBN structure is present at the hydrogels, and the benzene rings induce the orientation of the polymer in the ice crystals through π-π stacking during the freezing process; comparing the infrared spectra of PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels, it is found that PVA-OPD hydrogel has stronger CN stretching vibration peaks and -OH stretching vibration peaks, indicating that the hydrogels have greater interaction and stronger orientation structure;

[0064] Figure 4 XRD test was used to explore the hydrogel orientation structure from the perspective of crystallization. Among them, PVA hydrogel showed a strong diffraction peak of 1166% at 19°, indicating its higher crystallinity and stronger physical crosslinking. Compared with PVA hydrogel, the diffraction peak of the hydrogel introduced with aniline compounds at 19° was further enhanced, indicating its stronger crystallinity, because the interaction of the introduced aniline compounds was improved, making the polymer network structure tighter. Among them, the PVA-OPD hydrogel had the highest characteristic peak of 1185% at 19°, which was consistent with the results of FTIR.

[0065] Figure 5 The figures are the test results of the tensile and compressive properties of the hydrogels of Examples 1-5; wherein, a is the tensile stress-strain curve of PVA, PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels; b is the elastic modulus, toughness and maximum stress diagram; c is the compressive stress-strain curve; d is the stretching cycle of PVA-OPD hydrogel under different strains;

[0066] in, Figure 5 a shows that the maximum tensile stress of PVA hydrogel is 6 KPa, and the elongation at break is 334%. The tensile stress or elongation at break of the hydrogel introduced with aniline compounds is greatly improved. The tensile stress and elongation at break of PVA-OPD hydrogel are significantly enhanced, with a tensile stress of 20 KPa and an elongation at break of 416%. Further tests show that the elastic modulus and toughness of the hydrogel are Figure 5 b. Combination Figure 5 b It can be seen that the elastic modulus and toughness of PVA-OPD hydrogel are 3 KPa and 48 KJ / m 3 , 2 and 4 times that of PVA hydrogel, respectively;

[0067] Figure 5c shows that the maximum compressive stress of PVA hydrogel is 348 KPa, and the elongation at break is 77%, while the maximum compressive stress of PVA-OPD hydrogel is as high as 565 KPa, and the elongation at break is enhanced to 94%. It can be seen that the mechanical properties of PVA-OPD hydrogel are comprehensively improved, which is attributed to the fact that the amino groups of aniline compounds can form hydrogen bonds with PVA, increase the physical cross-linking density, and strengthen the polymer network, thereby improving the strength and toughness of the hydrogel;

[0068] Figure 5 d is the stretching cycle of PVA-OPD hydrogel under different strains. After five cycles in the strain range of 30%-200%, its stress tends to equilibrium; E elastic modulus, W toughness;

[0069] Figure 6 The fatigue resistance test results of the hydrogels of Examples 1-5 are shown in the figure. In the figure, a is the first tensile loading and unloading curve of PVA, PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels at 150% strain; b is the energy dissipation and tensile stress change diagram of PVA, PVA-ANI, PVA-OPD, PVA-MPD and PVA-PPD hydrogels; c is the tensile loading and unloading cycle curve of PVA-OPD hydrogel at 150% strain for 10 times; d is the energy dissipation and tensile stress change diagram of PVA-OPD hydrogel;

[0070] Figure 6 a-6b is the first tensile loading and unloading curve of different hydrogels under the condition of 150% elongation, and the hysteresis loop is analyzed to investigate its energy dissipation; the results show that the maximum stress at 150% strain corresponds to the data of the stress-strain curve, among which the PVA hydrogel has the largest hysteresis area and the energy dissipation is 23 KJ / m 3 After the introduction of aniline compounds, the energy dissipation of the hydrogels was reduced to varying degrees, showing low hysteresis and high elasticity, and having better recovery ability; among them, the energy dissipation of PVA-OPD hydrogel was the lowest at 14 KJ / m 3 , proving that OPD has the best regulatory effect;

[0071] Figure 6 c-6d is the test result of 10 stretching and loading and unloading cycles of PVA-OPD hydrogel; the results show that with the increase of stretching times, the energy dissipation of the first hysteresis loop is 14 KJ / m 3 The second energy dissipation drops sharply to 10 KJ / m 3 After the fourth loading, the curve is close to the previous unloading curve but does not completely overlap, and the energy dissipation is only 3.8 KJ / m 3And it remains basically unchanged; the reason is that some hydrogen bonds in the PVA-OPD hydrogel are broken during the loading process and will be restored after the unloading process, giving the hydrogel excellent anti-fatigue properties.

[0072] Combined with the above test results of the present invention, it can be known that in the present invention, aniline (ANI) derivatives are used as small molecule models, PVA hydrogel is used as a template, and the hydrogel is prepared by freezing and thawing; electron microscopy and microscopic observations show that the hydrogel regulated by aniline derivatives has an anisotropic structure, which is attributed to the dual effects of ANI molecules with both aromatic rings and hydrophilic groups forming hydrogen bonds with water molecules on the surface of ice crystals and π-π stacking of benzene rings, inducing water molecules to distribute in the optimal direction of the benzene ring in space, mediating the directional growth of ice crystals, and thus resulting in a highly oriented microstructure of the hydrogel. The results show that the anisotropic hydrogel regulated by OPD has the best performance, with a tensile stress of 20 KPa, a compressive stress of 565 KPa, an elongation at break of 416%, and an energy dissipation of 3.8 KJ / m 3 The prepared anisotropic hydrogel provides a new idea for the preparation of wearable sensors.

[0073] Although the present invention has been described in detail by reference to the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A method for preparing anisotropic hydrogel with aniline-regulated polymer network structure, characterized in that: The process is as follows: 18-20 mL of an aniline solvent with a concentration of 0.04-0.05 mol / L is taken, polyvinyl alcohol is dissolved at 93-97°C to obtain a polyvinyl alcohol solution with a concentration of 3-5 wt%; the solution is cooled to room temperature, then cooled at -20°C for 24 hours and thawed at room temperature for 4 hours to obtain a polyvinyl alcohol-based aniline hydrogel; The aniline solvent is prepared by adding water to one of aniline, o-phenylenediamine, m-phenylenediamine and p-phenylenediamine.

2. The method for preparing anisotropic hydrogel with aniline-regulated polymer network structure according to claim 1, characterized in that: 19 mL of 0.05 mol / L aniline solvent was mixed with 0.95 g of polyvinyl alcohol at 95°C to obtain a polyvinyl alcohol solution with a concentration of 4.75 wt%. The pH of the polyvinyl alcohol solution was 7.0±0.1.

Citation Information

Patent Citations

  • Functionalized shape anisotropy hydrogel particle embolization agent, and preparation method and application thereof

    CN113425887A

  • Hydrogel-attached nanofiber reinforcement

    CN113876999A