A method for smelting high carbon ferrochrome alloy

Through the hierarchical heat treatment of chromium ore and composite granulation technology, the impurity content in high-carbon ferrochromium alloy is reduced, the reducibility of carbon and the forging performance are improved, and the problems of high impurity content and insufficient reducibility of reducing agent in high-carbon ferrochromium alloy are solved. problem, meeting the performance requirements of special bearing steel.

CN118621165BActive Publication Date: 2024-10-22YINGKOU NEW TYPE SILICON PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114182.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-22
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The high impurity content and insufficient reducibility of the reducing agent in high-carbon ferrochromium alloys prevent its performance from meeting high requirements. Especially in the application of special bearing steels, the content requirements of Ti, V, and Si are stringent, which affects the structure and structure of the alloy. performance.

Method used

The chromium ore is subjected to graded heat treatment to remove SiO2, V2O5, TiO2 and other components, and the chromium oxide is purified. High-purity chromium oxide is mixed with hematite powder, and artificial graphite powder, delayed petroleum coke powder and carboxymethyl chitosan are added. Compounding, extrusion granulation or briquetting, adding carbon element in advance to improve the distribution uniformity and reducibility of carbon element, reduce the content of Ti, V and Si in the alloy, and improve the forging performance.

Benefits of technology

It significantly reduces the content of Ti, V and Si in the alloy, improves the reducibility and forging performance of carbon, meets the usage requirements of special bearing steel, and extends the service life of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

A smelting method for a high-carbon ferrochrome alloy belongs to the technical field of alloy smelting. The smelting method performs graded heat treatment on chromium ore, which can effectively remove impurities in the chromium ore, purify the chromium ore to obtain high-purity chromium oxide, and obtain high-purity carbon-reduced molten iron components; the high-purity chromium oxide and hematite powder are mixed, artificial graphite powder, delayed petroleum coke powder and carboxymethyl chitosan are mixed, and then compounded, extruded into granules or briquette, various carbon elements can be added to the smelting granular material or block material in advance, and the distribution is more uniform. During smelting, the reducibility of the carbon element is better, the carbon content in the alloy can be reduced to a certain extent, the forging performance is improved, and the use of carbon source can be saved; Ti in the high-carbon ferrochrome alloy is less than 0.01%, V is less than 0.02%, Si is less than 0.1%, the content of harmful impurities is greatly reduced, C is less than 7%, good forging performance can be maintained, and the use requirements of special bearing steel can be effectively met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy smelting, and in particular relates to a smelting method of a high-carbon ferrochrome alloy. Background Art

[0002] High carbon ferrochromium alloy is a commonly used stainless steel material. Stainless steel for different purposes has different performance requirements, and thus the requirements for the composition, content and structural characteristics of high carbon ferrochromium alloy are also different.

[0003] The composition, content and degree of metal oxide reduction of high-carbon ferrochrome alloy directly affect the structural characteristics and performance of stainless steel products. For example, if you want to achieve better performance when using high-carbon ferrochrome alloy to prepare ball bearing steel, you need to reduce the impurity content as much as possible. For example, components such as Ti, V, and Si will affect the difficulty of the production process and the alloy structure, affect the hardness and brittleness of the product, coercive force, etc., and shorten the service life of the alloy. Especially for special bearing steel, the requirements for the content of titanium and silicon in high-carbon ferrochrome alloy are more stringent. The Ti content must be less than 0.03%, the V content must be less than 0.05%, and the Si content must be less than 0.3%. In addition, the carbon reduction ability in the high-carbon ferrochrome alloy must be high to prepare high-purity high-carbon ferrochrome alloy.

[0004] The composition and content of high carbon ferrochrome alloy are mainly affected by the quality of raw materials and auxiliary materials. At present, most of the raw materials and auxiliary materials contain high content of impurity elements, which inevitably introduce various high-content impurities. Therefore, in order to reduce the impurity content of high carbon ferrochrome alloy, it is necessary to improve the smelting method and parameter control; in addition, the reducibility of reducing agents such as carbon and silica to metal oxides also affects the alloy structure and determines the performance of the alloy. Summary of the invention

[0005] The high content of harmful impurities in the existing high-carbon ferrochrome alloy and the reducibility of the reducing agent affect the alloy structure, so that the performance of the current high-carbon ferrochrome alloy cannot meet higher requirements. The present invention provides a smelting method of high-carbon ferrochrome alloy, which performs graded heat treatment on chromium ore, can effectively remove SiO2, V2O5, TiO2 components and other low-temperature hot-melting components and infusible components above 2500°C in the chromium ore, purify the chromium ore to obtain high-purity chromium oxide, and obtain high-purity carbon-reduced molten iron components; mix the high-purity chromium oxide and hematite powder, mix artificial graphite powder, delayed petroleum coke powder and carboxymethyl chitosan, and then compound, extrude granulate or briquette, which can be used in Adding various carbon elements to the smelting granular or block materials in advance makes the distribution of various components more uniform. During smelting, the reducibility of carbon elements is better, which can reduce the carbon content in the alloy to a certain extent and improve the forging performance; compound granulation or briquetting can also relatively reduce the amount of carbon raw materials used; Ti < 0.01%, V < 0.02%, Si < 0.1% in the prepared high-carbon ferrochrome alloy, greatly reducing the content of harmful impurities, 6% < C < 7%, can maintain good forging performance, and effectively meet the use requirements of special bearing steel. The specific technical scheme is as follows:

[0006] A smelting method for high carbon ferrochrome alloy, the smelting method comprising the following steps:

[0007] S1, raw material preparation:

[0008] Prepare materials by weight: 400-500 parts of chromium ore, 20-60 parts of hematite powder, 30-50 parts of artificial graphite powder, 40-60 parts of delayed petroleum coke powder, 10-20 parts of carboxymethyl chitosan, and 3-5 parts of calcined petroleum coke powder;

[0009] S2, Raw material processing:

[0010] The chromium ore is crushed into a crushed stone body, and is put into a furnace, the highest temperature of the furnace is 1420℃~1500℃, and furnace water I flows out, and furnace water I is collected as a by-product; the slag I is continuously put into the furnace, the highest temperature of the furnace rises to 1600℃~1800℃, and furnace water II flows out, and furnace water II is collected, and calcined petroleum coke powder is added to furnace water II to obtain carbon-enhanced furnace water II, and carbon-enhanced furnace water II is cast and cooled into an ingot for standby use; the slag II is continuously put into the furnace, the highest temperature of the furnace rises to 1980℃~2150℃, and furnace water III flows out, and furnace water III is collected as a by-product; the slag III is continuously put into the furnace, the highest temperature of the furnace rises to 2300℃~2500℃, and furnace water IV flows out, and furnace water IV is collected, cooled, crushed, and material A is obtained for standby use; slag IV is produced as a by-product;

[0011] S3, Mixing and Blocking:

[0012] The material A and the hematite powder are mixed evenly to obtain a mixture B, and the artificial graphite powder, the delayed petroleum coke powder and the carboxymethyl chitosan are mixed evenly to obtain a mixture C; the mixture B and the mixture C are mixed evenly to obtain a composite material D, and water is added to the composite material D to mix, extrude and granulate, and dry to obtain a granular material; or water is added to the composite material D to mix, briquette, and dry to obtain a block material;

[0013] S4, Smelting:

[0014] Put the granular material or block material into the ore-melting furnace, then put in the slag-making agent, heat it to 1000℃~1200℃ and smelt it for 0.5h~1h, heat it to 1350℃~1450℃ and smelt it for 1.5h~2h, heat it to 1600℃~1700℃ and smelt it for 5h~6h, and obtain high-carbon ferrochrome alloy furnace water; the produced smelting slag is used as a by-product;

[0015] S4, Casting:

[0016] The high-carbon ferrochrome alloy is casted with furnace water and post-processed to obtain the high-carbon ferrochrome alloy; in the high-carbon ferrochrome alloy, Cr>52%, 6%<C<7%, Ti<0.01%, V<0.02%, Si<0.1%, by mass content.

[0017] In S1 of the above smelting method, the chromium ore is chromite, and its mass content is 38% to 43% Cr2O3, 15% to 27% Fe2O3, 10% to 20% MgO, 7% to 12% Al2O3, 7% to 10% SiO2, 0.2% to 0.5% V2O5, 0.2% to 0.6% TiO2, and the remainder is unavoidable impurities.

[0018] In S1 of the above smelting method, the particle size range of the hematite powder is 0.1 mm to 2 mm.

[0019] In S1 of the above smelting method, the particle size range of the artificial graphite powder is 50 μm to 800 μm; the artificial graphite powder is powder obtained by crushing discarded steelmaking graphite electrodes after peeling.

[0020] In S1 of the above smelting method, the particle size range of the delayed petroleum coke powder is 5 μm to 500 μm.

[0021] In S1 of the above smelting method, the particle size range of the carboxymethyl chitosan is below 500 μm.

[0022] In S1 of the above smelting method, the particle size range of the calcined petroleum coke powder is 50 μm to 800 μm.

[0023] In S2 of the above smelting method, the particle size range of the crushed stone is 5 mm to 30 mm; the particle size range of the material A is 0.1 mm to 2 mm.

[0024] In S2 of the above smelting method, the diameter of the ingot is 10 mm to 30 mm.

[0025] In S3 of the above smelting method, the amount of water added does not exceed 15% of the mass of the composite material D.

[0026] In S3 of the above smelting method, the particle size of the granular material is 5mm to 15mm; the diameter of the block material is 15mm to 30mm.

[0027] In S4 of the above smelting method, the ingot obtained in S2 is also put into the submerged arc furnace; the ingot is put into the furnace before the slag-forming agent.

[0028] In S4 of the above smelting method, the slag-forming agent is bluestone; or the slag-forming agent is a mixture of bluestone and smelting slag.

[0029] The mixing mass ratio of the bluestone and the smelting slag is bluestone:smelting slag=100:(20-30).

[0030] In S2 of the above smelting method, the furnace is a blast furnace or a vertical furnace.

[0031] Compared with the prior art, the smelting method of a high carbon ferrochrome alloy of the present invention has the following beneficial effects:

[0032] 1. The method of the present invention crushes chromium ore into crushed stone and performs graded heat treatment, which can effectively remove SiO2, V2O5, TiO2 components and other low-temperature hot-melting components and infusible components above 2500°C in the chromium ore, purify the chromium ore to obtain high-purity chromium oxide, i.e., material A; and obtain high-purity carbon-reduced molten iron components, which are helpful for subsequent smelting and reduce alloy impurities.

[0033] 2. The method of the present invention mixes high-purity chromium oxide and hematite powder, and the hematite powder is used to adjust the chromium iron content without introducing too many impurities; artificial graphite powder, delayed petroleum coke powder and carboxymethyl chitosan are mixed, and then compounded, extruded granulated or briquette, so that various carbon elements can be added to the smelting granular material or block material in advance, and the distribution of each carbon source component is more uniform. During smelting, the reducibility of carbon elements is better, which can reduce the carbon content in the alloy to a certain extent and improve the forging performance. In addition, compound granulation or briquetting can relatively reduce the amount of carbon source used.

[0034] 3. The method of the present invention adopts a variety of carbon sources, including artificial graphite powder, delayed petroleum coke powder, carboxymethyl chitosan and calcined petroleum coke powder. The properties of various carbon sources are different. Artificial graphite powder has better reducibility under high temperature conditions above 1600°C. Delayed petroleum coke powder itself has a certain viscosity. When used with carboxymethyl chitosan and water, it has good adhesion, reduces the amount of water used, can be well granulated and briquette, maintains good hardness, and will not easily loosen; and carboxymethyl chitosan carbonizes under high temperature environment, which can promote The reduction of oxides is further carried out; the delayed petroleum coke powder is further carbonized at 1000℃~1200℃, and has better reducing property to oxides at 1350℃~1450℃, and can quickly reduce Cr2O3 to Cr7C3; the various carbon sources are used in combination and integrated into the mineral particles and blocks, with better reducing ability and more thorough and uniform reduction. Good reduction effect can be achieved by smelting at 1600℃~1700℃ for 5h~6h, which greatly saves the smelting time at 1600℃~1700℃ and reduces energy consumption.

[0035] 4. In the alloy prepared by the method of the present invention, Ti is less than 0.01%, V is less than 0.02%, and Si is less than 0.1%, which greatly reduces the content of harmful impurities. When smelted at 1600℃~1700℃, better reducibility can be achieved, so that C in the alloy is less than 7%, good forging performance can be maintained, and the use requirements of special bearing steel can be effectively met. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited to these embodiments:

[0037] Embodiment 1: A method for smelting a high carbon ferrochrome alloy, the smelting method comprising the following steps:

[0038] S1, raw material preparation:

[0039] Prepare materials by mass: 450 parts of chromium ore, 50 parts of hematite powder, 40 parts of artificial graphite powder, 50 parts of delayed petroleum coke powder, 15 parts of carboxymethyl chitosan, and 4 parts of calcined petroleum coke powder;

[0040] Among them, the chromium ore is chromite, with a mass content of 40.2% Cr2O3, 22.8% Fe2O3, 14.3% MgO, 9.4% Al2O3, 9.6% SiO2, 0.4% V2O5, 0.5% TiO2, and the remainder is inevitable impurities. The particle size range of hematite powder is 0.1mm~2mm. The particle size range of artificial graphite powder is 50μm~800μm; artificial graphite powder is the powder of discarded steelmaking graphite electrodes after peeling. The particle size range of delayed petroleum coke powder is 5μm~500μm. The particle size range of carboxymethyl chitosan is below 500μm. The particle size range of calcined petroleum coke powder is 50μm~800μm.

[0041] S2, Raw material processing:

[0042] The chromium ore is crushed into a crushed stone body with a particle size range of 5mm to 30mm, and is put into a blast furnace. The maximum temperature of the furnace is 1450°C, and furnace water I flows out. The furnace water I is collected as a by-product; the slag I is continuously put into the furnace, the maximum temperature of the furnace rises to 1700°C, and furnace water II flows out. The furnace water II is collected, and calcined petroleum coke powder is added to the furnace water II to obtain carbon-enhanced furnace water II. The carbon-enhanced furnace water II is cast and cooled into an ingot with a diameter of 10mm to 30mm for standby use; the slag II is continuously put into the furnace, the maximum temperature of the furnace rises to 2100°C, and furnace water III flows out. The furnace water III is collected as a by-product; the slag III is continuously put into the furnace, the maximum temperature of the furnace rises to 2400°C, and furnace water IV flows out. The furnace water IV is collected, cooled, crushed and classified into a particle size range of 0.1mm to 2mm, and material A is obtained for standby use; slag IV is produced as a by-product;

[0043] S3, Mixing and Blocking:

[0044] The material A and the hematite powder are mixed evenly to obtain a mixture B, and the artificial graphite powder, the delayed petroleum coke powder and the carboxymethyl chitosan are mixed evenly to obtain a mixture C; the mixture B and the mixture C are mixed evenly to obtain a composite material D, and 13% by weight of water is added to the composite material D, and the mixture is mixed, extruded and granulated, and dried to obtain a granular material with a particle size of 5 mm to 15 mm;

[0045] S4, Smelting:

[0046] Put the pellets into a submerged arc furnace, put ingots, and then put bluestone slag-making agent, heat to 1100°C for smelting for 0.5h, heat to 1400°C for smelting for 1.5h, heat to 1650°C for smelting for 5h, and obtain high-carbon ferrochrome alloy furnace water; the generated smelting slag is used as a by-product;

[0047] S4, Casting:

[0048] The high carbon ferrochrome alloy is casted with furnace water and post-processed to obtain the high carbon ferrochrome alloy. The component contents of the high carbon ferrochrome alloy prepared in this embodiment are detected, as shown in Table 1.

[0049] Embodiment 2: A method for smelting a high carbon ferrochrome alloy, the smelting method comprising the following steps:

[0050] S1, raw material preparation:

[0051] Prepare materials by mass: 500 parts of chromium ore, 60 parts of hematite powder, 50 parts of artificial graphite powder, 60 parts of delayed petroleum coke powder, 20 parts of carboxymethyl chitosan, and 5 parts of calcined petroleum coke powder;

[0052] Among them, the chromium ore is chromite, with a mass content of 39.8% Cr2O3, 21.6% Fe2O3, 17.4% MgO, 10.5% Al2O3, 7.6% SiO2, 0.3% V2O5, 0.5% TiO2, and the remainder is inevitable impurities. The particle size range of hematite powder is 0.1mm~2mm. The particle size range of artificial graphite powder is 50μm~800μm; artificial graphite powder is the powder of discarded steelmaking graphite electrodes after peeling. The particle size range of delayed petroleum coke powder is 5μm~500μm. The particle size range of carboxymethyl chitosan is below 500μm. The particle size range of calcined petroleum coke powder is 50μm~800μm.

[0053] S2, Raw material processing:

[0054] The chromium ore is crushed into a crushed stone body with a particle size range of 5mm to 30mm, and is put into a blast furnace. The maximum temperature of the furnace is 1500℃, and furnace water I flows out. The furnace water I is collected as a by-product; the slag I is continuously put into the furnace, and the maximum temperature of the furnace is raised to 1800℃, and furnace water II flows out. The furnace water II is collected, and calcined petroleum coke powder is added to the furnace water II to obtain carbon-enhanced furnace water II. The carbon-enhanced furnace water II is cast and cooled into an ingot with a diameter of 10mm to 30mm for standby use; the slag II is continuously put into the furnace, and the maximum temperature of the furnace is raised to 2150℃, and furnace water III flows out. The furnace water III is collected as a by-product; the slag III is continuously put into the furnace, and the maximum temperature of the furnace is raised to 2500℃, and furnace water IV flows out. The furnace water IV is collected, cooled, crushed and classified into a particle size range of 0.1mm to 2mm, and material A is obtained for standby use; slag IV is produced as a by-product;

[0055] S3, Mixing and Blocking:

[0056] The material A and the hematite powder are mixed evenly to obtain a mixture B, and the artificial graphite powder, the delayed petroleum coke powder and the carboxymethyl chitosan are mixed evenly to obtain a mixture C; the mixture B and the mixture C are mixed evenly to obtain a composite material D, and no more than 12% by weight of water is added to the composite material D, and the mixture is mixed, extruded and granulated, and dried to obtain a granular material with a particle size of 5 mm to 15 mm;

[0057] S4, Smelting:

[0058] The pellets are put into a submerged arc furnace, an ingot is cast, and a slag-making agent is added. The temperature is raised to 1200° C. for smelting for 1 hour, the temperature is raised to 1450° C. for smelting for 2 hours, and the temperature is raised to 1700° C. for smelting for 6 hours to obtain high-carbon ferrochrome alloy furnace water; the smelting slag produced is used as a by-product;

[0059] The slag-forming agent is a mixture of bluestone and smelting slag, and the mixing mass ratio is bluestone: smelting slag = 100:25.

[0060] S4, Casting:

[0061] The high carbon ferrochrome alloy is casted with furnace water and post-processed to obtain the high carbon ferrochrome alloy. The component contents of the high carbon ferrochrome alloy prepared in this embodiment are detected, as shown in Table 1.

[0062] Embodiment 3: A method for smelting a high carbon ferrochrome alloy, the smelting method comprising the following steps:

[0063] S1, raw material preparation:

[0064] Prepare materials by mass: 490 parts of chromium ore, 20 parts of hematite powder, 45 parts of artificial graphite powder, 55 parts of delayed petroleum coke powder, 15 parts of carboxymethyl chitosan, and 4 parts of calcined petroleum coke powder;

[0065] Among them, the chromium ore is chromite, with a mass content of 38.0% Cr2O3, 27.0% Fe2O3, 10.0% MgO, 12.0% Al2O3, 7.0% SiO2, 0.5% V2O5, 0.6% TiO2, and the remainder is inevitable impurities. The particle size range of hematite powder is 0.1mm~2mm. The particle size range of artificial graphite powder is 50μm~800μm; artificial graphite powder is the powder of discarded steelmaking graphite electrodes after peeling. The particle size range of delayed petroleum coke powder is 5μm~500μm. The particle size range of carboxymethyl chitosan is below 500μm. The particle size range of calcined petroleum coke powder is 50μm~800μm.

[0066] S2, Raw material processing:

[0067] The chromium ore is crushed into a crushed stone body with a particle size range of 5mm to 30mm, and is put into a blast furnace. The maximum temperature of the furnace is 1460°C, and furnace water I flows out. The furnace water I is collected as a by-product; the slag I is continuously put into the furnace, and the maximum temperature of the furnace rises to 1650°C, and furnace water II flows out. The furnace water II is collected, and calcined petroleum coke powder is added to the furnace water II to obtain carbon-enhanced furnace water II. The carbon-enhanced furnace water II is cast and cooled into an ingot with a diameter of 10mm to 30mm for standby use; the slag II is continuously put into the furnace, and the maximum temperature of the furnace rises to 2000°C, and furnace water III flows out. The furnace water III is collected as a by-product; the slag III is continuously put into the furnace, and the maximum temperature of the furnace rises to 2350°C, and furnace water IV flows out. The furnace water IV is collected, cooled, crushed and classified into a particle size range of 0.1mm to 2mm, and material A is obtained for standby use; slag IV is produced as a by-product;

[0068] S3, Mixing and Blocking:

[0069] The material A and the hematite powder are mixed evenly to obtain a mixture B, and the artificial graphite powder, the delayed petroleum coke powder and the carboxymethyl chitosan are mixed evenly to obtain a mixture C; the mixture B and the mixture C are mixed evenly to obtain a composite material D, and 15% by weight of water is added to the composite material D, and the mixture is mixed, extruded and granulated, and dried to obtain a granular material with a particle size of 5 mm to 15 mm;

[0070] S4, Smelting:

[0071] The pellets are put into a submerged arc furnace, an ingot is cast, and a slag-making agent is added. The temperature is raised to 1050°C for smelting for 1 hour, the temperature is raised to 1380°C for smelting for 1.5 hours, and the temperature is raised to 1600°C for smelting for 6 hours to obtain high-carbon ferrochrome alloy furnace water; the smelting slag produced is used as a by-product;

[0072] The slag-forming agent is a mixture of bluestone and smelting slag, and the mixing mass ratio is bluestone: smelting slag = 100:20.

[0073] S4, Casting:

[0074] The high carbon ferrochrome alloy is casted with furnace water and post-processed to obtain the high carbon ferrochrome alloy. The component contents of the high carbon ferrochrome alloy prepared in this embodiment are detected, as shown in Table 1.

[0075] Embodiment 4: A method for smelting a high carbon ferrochrome alloy, the smelting method comprising the following steps:

[0076] S1, raw material preparation:

[0077] Prepare materials by mass: 400 parts of chromium ore, 40 parts of hematite powder, 30 parts of artificial graphite powder, 10 parts of delayed petroleum coke powder, 12 parts of carboxymethyl chitosan, and 3 parts of calcined petroleum coke powder;

[0078] Among them, the chromium ore is chromite, with a mass content of 43.0% Cr2O3, 15.0% Fe2O3, 20.0% MgO, 7.0% Al2O3, 10.0% SiO2, 0.2% V2O5, 0.2% TiO2, and the remainder is inevitable impurities. The particle size range of hematite powder is 0.1mm~2mm. The particle size range of artificial graphite powder is 50μm~800μm; artificial graphite powder is the powder of discarded steelmaking graphite electrodes after peeling. The particle size range of delayed petroleum coke powder is 5μm~500μm. The particle size range of carboxymethyl chitosan is below 500μm. The particle size range of calcined petroleum coke powder is 50μm~800μm.

[0079] S2, Raw material processing:

[0080] The chromium ore is crushed into a crushed stone body with a particle size range of 5mm to 30mm, and is put into a vertical furnace. The maximum temperature of the furnace is 1420℃, and furnace water I flows out. The furnace water I is collected as a by-product; the slag I is continuously put into the furnace, and the maximum temperature of the furnace is raised to 1600℃, and furnace water II flows out. The furnace water II is collected, and calcined petroleum coke powder is added to the furnace water II to obtain carbon-enhanced furnace water II. The carbon-enhanced furnace water II is cast and cooled into an ingot with a diameter of 10mm to 30mm for standby use; the slag II is continuously put into the furnace, and the maximum temperature of the furnace is raised to 1980℃, and furnace water III flows out. The furnace water III is collected as a by-product; the slag III is continuously put into the furnace, and the maximum temperature of the furnace is raised to 2300℃, and furnace water IV flows out. The furnace water IV is collected, cooled, crushed and classified into a particle size range of 0.1mm to 2mm, and material A is obtained for standby use; slag IV is produced as a by-product;

[0081] S3, Mixing and Blocking:

[0082] The material A and the hematite powder are mixed evenly to obtain a mixture B, and the artificial graphite powder, the delayed petroleum coke powder and the carboxymethyl chitosan are mixed evenly to obtain a mixture C; the mixture B and the mixture C are mixed evenly to obtain a composite material D, and 10% by weight of water is added to the composite material D, mixed and pressed into blocks, and dried to obtain a block material with a diameter of 15 mm to 30 mm;

[0083] S4, Smelting:

[0084] Put the block material into the ore-fired furnace, put ingots, and then put slag-making agent, heat to 1000℃ and smelt for 0.5h, heat to 1350℃ and smelt for 1.5h, heat to 1600℃ and smelt for 5h, and obtain high-carbon ferrochrome alloy furnace water; the generated smelting slag is used as a by-product;

[0085] The slag-forming agent is a mixture of bluestone and smelting slag, and the mixing mass ratio is bluestone: smelting slag = 100:30.

[0086] S4, Casting:

[0087] The high carbon ferrochrome alloy is casted with furnace water and post-processed to obtain the high carbon ferrochrome alloy. The component contents of the high carbon ferrochrome alloy prepared in this embodiment are detected, as shown in Table 1.

[0088] Preparation Comparative Example 1:

[0089] The chromium ore is the chromium ore of Example 1, and the chromium ore is not subjected to S2 treatment. The chromium ore is crushed and classified to a particle size range of 0.1 mm to 2 mm, and then mixed to form blocks; the other steps and parameters are the same as those of Example 1. (The chromium ore is the chromium ore of Example 1)

[0090] Preparation Comparative Example 2:

[0091] The chromium ore is the chromium ore of Example 1. In S2, furnace water IV is collected, cooled, crushed and classified into a particle size range of 5mm to 15mm to obtain material A; hematite is crushed into granular materials of 5mm to 15mm; by mass, 450 parts of chromium ore granular materials, 50 parts of hematite granular materials, 40 parts of artificial graphite powder, 50 parts of delayed petroleum coke powder, 15 parts of carboxymethyl chitosan, and 4 parts of calcined petroleum coke powder are directly put into the furnace for smelting; the temperature is directly raised to 1650°C for smelting for 6h; other steps and parameters are the same as in Example 1.

[0092] Preparation Comparative Example 3:

[0093] The chromium ore used is the chromium ore of Example 1, and the chromium ore is not subjected to S2 treatment. The chromium ore and hematite are crushed into particles of 5 mm to 15 mm. By mass, 450 parts of chromium ore, 50 parts of hematite powder and 109 parts of calcined petroleum coke powder are directly heated to 1650° C. and smelted for 6 hours. Other steps and parameters are the same as in Example 1.

[0094] The chromium ore component detection method of the above embodiment is carried out according to "Determination of the content of magnesium, aluminum, silicon, calcium, titanium, vanadium, chromium, manganese, iron and nickel in chromium ore - Wavelength dispersive X-ray fluorescence spectrometry GB / T 24231-2009".

[0095] The component contents of the high carbon ferrochromium alloys prepared in the above-mentioned embodiments and comparative examples were detected, as shown in Table 1.

[0096] Table 1 Component content test results of high carbon ferrochromium alloy

[0097]

[0098] It can be seen from the component contents of the above-mentioned high-carbon ferrochrome alloy that the high-carbon ferrochrome alloy prepared in Examples 1 to 4 has extremely low Si, V, and Ti contents, and the degree of carbon reduction to oxides is high, the carbon content is low, and the forging performance can be improved. The high-carbon ferrochrome alloy prepared in Comparative Examples 1 to 3 has a relatively high carbon content and a relatively poor degree of reduction to oxides. The high carbon content will affect the forging performance to a certain extent. In addition, the high-carbon ferrochrome alloys in Comparative Examples 1 and 3 have high Si, V, and Ti contents, which do not meet the use requirements of special bearing steels. This shows that the raw material processing of chromite can effectively reduce the content of harmful impurities, and the use of composite granulation or briquetting technology can also reduce the harmful impurities of the product to a certain extent; at the same time, the use of composite granulation or briquetting technology can improve the smelting distribution of carbon elements in the alloy components, the reduction of oxide components is better, the alloy components are more uniform, and the carbon content is lower, which helps to improve the forging performance.

Claims

1. A method for smelting a high carbon ferrochrome alloy, characterized in that: The smelting method comprises the following steps: S1, raw material preparation: Prepare materials by weight: 400-500 parts of chromium ore, 20-60 parts of hematite powder, 30-50 parts of artificial graphite powder, 40-60 parts of delayed petroleum coke powder, 10-20 parts of carboxymethyl chitosan, and 3-5 parts of calcined petroleum coke powder; The chromium ore is chromite, and its mass content is 38% to 43% Cr2O3, 15% to 27% Fe2O3, 10% to 20% MgO, 7% to 12% Al2O3, 7% to 10% SiO2, 0.2% to 0.5% V2O5, 0.2% to 0.6% TiO2, and the balance is inevitable impurities; S2, Raw material processing: The chromium ore is crushed into a crushed stone body, and is put into a furnace, the highest temperature of the furnace is 1420℃~1500℃, and furnace water I flows out, and furnace water I is collected as a by-product; the slag I is continuously put into the furnace, the highest temperature of the furnace rises to 1600℃~1800℃, and furnace water II flows out, and furnace water II is collected, and calcined petroleum coke powder is added to furnace water II to obtain carbon-enhanced furnace water II, and carbon-enhanced furnace water II is cast and cooled into an ingot for standby use; the slag II is continuously put into the furnace, the highest temperature of the furnace rises to 1980℃~2150℃, and furnace water III flows out, and furnace water III is collected as a by-product; the slag III is continuously put into the furnace, the highest temperature of the furnace rises to 2300℃~2500℃, and furnace water IV flows out, and furnace water IV is collected, cooled, crushed, and material A is obtained for standby use; slag IV is produced as a by-product; S3, Mixing and Blocking: The material A and the hematite powder are mixed evenly to obtain a mixture B, and the artificial graphite powder, the delayed petroleum coke powder and the carboxymethyl chitosan are mixed evenly to obtain a mixture C; the mixture B and the mixture C are mixed evenly to obtain a composite material D, and water is added to the composite material D to mix, extrude and granulate, and dry to obtain a granular material; or water is added to the composite material D to mix, briquette, and dry to obtain a block material; S4, Smelting: Put the granular material or block material into the ore-melting furnace, put ingot, and then put in slag-making agent, heat it to 1000℃~1200℃ and smelt it for 0.5h~1h, heat it to 1350℃~1450℃ and smelt it for 1.5h~2h, heat it to 1600℃~1700℃ and smelt it for 5h~6h, and obtain high-carbon ferrochrome alloy furnace water; the generated smelting slag is used as a by-product; S4, Casting: The high-carbon ferrochrome alloy is casted with furnace water and post-processed to obtain the high-carbon ferrochrome alloy; in the high-carbon ferrochrome alloy, Cr>52%, 6%<C<7%, Ti<0.01%, V<0.02%, Si<0.1%, by mass content.

2. The method for smelting a high carbon ferrochrome alloy according to claim 1, characterized in that: In S1, the particle size range of the hematite powder is 0.1mm-2mm; the particle size range of the artificial graphite powder is 50μm-800μm; the particle size range of the delayed petroleum coke powder is 5μm-500μm; the particle size range of the carboxymethyl chitosan is below 500μm; the particle size range of the calcined petroleum coke powder is 50μm-800μm.

3. The smelting method of a high carbon ferrochrome alloy according to claim 1, characterized in that: In S1, the artificial graphite powder is powder obtained by crushing discarded steelmaking graphite electrodes after peeling.

4. The smelting method of a high carbon ferrochrome alloy according to claim 1, characterized in that: In S2, the particle size range of the crushed stone is 5 mm to 30 mm; the particle size range of the material A is 0.1 mm to 2 mm.

5. The method for smelting a high carbon ferrochrome alloy according to claim 1, characterized in that: In S2, the diameter of the ingot is 10 mm to 30 mm.

6. The method for smelting a high carbon ferrochrome alloy according to claim 1, characterized in that: In S3, the amount of water added does not exceed 15% of the mass of the composite material D.

7. The method for smelting a high carbon ferrochrome alloy according to claim 1, characterized in that: In S3, the particle size of the granular material is 5 mm to 15 mm; the diameter of the block material is 15 mm to 30 mm.

8. The method for smelting a high carbon ferrochrome alloy according to claim 1, characterized in that: In S4, the slag-forming agent is bluestone; or the slag-forming agent is a mixture of bluestone and smelting slag, and the mixing mass ratio of the bluestone and the smelting slag is bluestone:smelting slag=100:(20-30).