A resin-modified dual-speed magnesium phosphate cement anchor and its use method

By using a dual-speed anchoring agent of modified resin and magnesium phosphate cement in coal mining, the problem of structural stability of the anchoring agent in a water environment is solved, full-length anchoring and high-strength anchoring effects are achieved, and the safety of coal mining is ensured. sex and efficiency.

CN118637885BActive Publication Date: 2024-10-22SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125982.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-22
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

During the coal mining process, the structural integrity and load-bearing capacity of the anchoring agent are reduced when it encounters water, causing the surrounding rock anchoring structure to become unstable and unable to achieve full-length prestressed anchoring, resulting in the occurrence of ineffective anchoring sections.

Method used

A dual-speed magnesium phosphate cement anchor based on resin modification is used, through a combination of fast-setting slurry and slow-setting slurry, using modified unsaturated polyester resin, dead-burned magnesium oxide powder, mineral admixtures and phosphates, etc. components to form a dual-speed setting structure to enhance anchoring strength and water resistance.

Benefits of technology

It achieves the normal development of anchoring strength in a water-bearing environment, enhances the anchoring force, ensures the stability and safety of the surrounding rock of the tunnel, and avoids instability of the anchoring structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637885B_ABST
    Figure CN118637885B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of cement materials, and specifically discloses a resin-modified dual-speed magnesium phosphate cement anchor and a method of using the same. The anchor comprises a fast-setting slurry and a slow-setting slurry, both of which comprise components A and B. Component A comprises: modified unsaturated polyester resin, dead-burned magnesium oxide powder, mineral admixture, fiber, water reducer, fine aggregate, polymer rubber powder, and water. Component B comprises: resin curing agent, phosphate, retarder, and water, and the content of the retarder in the fast-setting slurry is lower than that in the slow-setting slurry. The preparation method of the modified unsaturated polyester resin is as follows: unsaturated polyester resin, accelerator, dimethylaniline, silane coupling agent, and nano-SiO2 are mixed and heated and stirred to obtain the product. The amount of accelerator used in the modified unsaturated polyester resin in the fast-setting slurry is higher than that in the slow-setting slurry. The anchor of the present invention has the characteristics of dual-speed setting, full-length anchoring, high strength, strong anchoring force, and normal development of strength in a water-containing environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement materials, and in particular to a resin-modified dual-speed magnesium phosphate cement anchoring agent and a use method thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The geological conditions of my country's coal are complex and coal accidents occur frequently, so it is crucial to ensure the safety and efficiency of coal resource mining. Statistics show that tunnels supported by anchor rods account for more than two-thirds of the tunnel support in the country. However, due to the constraints of the occurrence conditions, the influence of water (water used for construction and production, underground seepage water, environmental humidity, etc.) in the coal mining process is difficult to avoid. Water is one of the main factors affecting the stability of the tunnel surrounding rock anchoring structure. If effective support and control measures are not taken, the structural integrity and bearing capacity of the anchoring agent will decrease rapidly after encountering water, and even non-condensation will occur, weakening the coupling ability between the surrounding rock and the support material, resulting in the overall instability of the tunnel surrounding rock anchoring structure, and then inducing engineering disasters.

[0004] Magnesium phosphate material (MPC) is a special cementitious material formed by heavy-burned magnesium oxide and phosphate in an appropriate proportion. After adding water, it undergoes an acid-base neutralization reaction to solidify and harden. Magnesium phosphate material has the advantages of fast solidification and hardening, high early strength, good bonding performance, good volume stability, and can undergo phosphating reaction with the surface of steel to increase corrosion resistance. At present, magnesium phosphate cement has been used as an anchoring agent for anchor rods and has achieved good anchoring effects. However, the inventors have found that in areas with water seepage and water sprinkling, the performance of ordinary resin anchoring agents is reduced due to the effect of water, making it difficult to achieve full-length prestressed anchoring of the anchor rod, resulting in the appearance of a large number of invalid anchoring sections. Summary of the invention

[0005] In view of the above problems, the present invention provides a resin-modified dual-speed magnesium phosphate cement anchoring agent and a method for using the same. The anchoring agent has the characteristics of dual-speed setting, full-length anchoring, high strength, strong anchoring force, and normal strength development in a water-containing environment. Specifically, the technical solution of the present invention is as follows.

[0006] First, the present invention provides a resin-modified dual-speed magnesium phosphate cement anchor, comprising: a fast-setting slurry and a slow-setting slurry, the mass ratio of the two being 0.5-1:1. Both of the two slurries comprise component A and component B:

[0007] The component A comprises: 10 to 135 parts by weight of modified unsaturated polyester resin, 30 to 90 parts by weight of dead-burned magnesium oxide powder, 10 to 50 parts by weight of mineral admixture, 1 to 5 parts by weight of fiber, 1.5 to 3 parts by weight of water reducer, 50 to 135 parts by weight of fine aggregate, 1 to 10 parts by weight of polymer rubber powder, and 10 to 25 parts by weight of water.

[0008] The B component includes: 0.2-4 parts by weight of a resin curing agent, 18-45 parts by weight of a phosphate, 0-3 parts by weight of a retarder, and 5-8 parts by weight of water. The amount of the retarder in the fast-setting slurry is 25-50% of the amount of the retarder in the slow-setting slurry, and the retarder in the slow-setting slurry is not less than 1.2 parts by weight to ensure that the fast-setting slurry solidifies faster than the slow-setting slurry.

[0009] The modified unsaturated polyester resin is prepared by the following method: unsaturated polyester resin, accelerator, dimethylaniline, silane coupling agent and nano-SiO2 are mixed and heated and stirred to obtain the modified unsaturated polyester resin. The amount of the accelerator of the modified unsaturated polyester resin in the slow-setting slurry is 25-50% of the amount of the accelerator in the fast-setting slurry, so as to ensure that the fast-setting slurry coagulates faster than the slow-setting slurry to form an initial anchoring force, so as to facilitate the subsequent application of prestress to the anchor rod.

[0010] Furthermore, the ratios of the unsaturated polyester resin, accelerator, dimethylaniline, silane coupling agent and nano-SiO2 are 10-135 parts by weight: 0.01-1.5 parts by weight: 0.1-2 parts by weight: 0.1-2 parts by weight: 1-8 parts by weight.

[0011] Furthermore, the accelerator includes at least one of benzoyl peroxide, cyclohexanone peroxide, formic acid, ethylenediamine, triethanolamine, etc. The accelerator can provide active hydrogen, initiate free radicals, reduce the adsorption of free radicals, etc., thereby accelerating the curing speed and efficiency of the unsaturated polyester resin by shortening the gel time and hardening time of the resin. In addition, the accelerator can also improve the compressive strength, hardness, wear resistance and chemical corrosion resistance of the unsaturated polyester resin.

[0012] Furthermore, the silane coupling agent includes at least one of KH550, KH560, KH570, KH792, DL602 and the like.

[0013] Furthermore, the heating and stirring is performed at a temperature of 50-80° C. and for a time of 100-300 min.

[0014] Further, the fiber includes at least one of basalt fiber, polyvinyl alcohol fiber, steel fiber, carbon fiber, glass fiber, polypropylene fiber, etc. Optionally, the length of the fiber is 3 to 12 mm. The fiber helps to improve the strength of the anchoring agent and the stability before coagulation.

[0015] Furthermore, the water reducer includes at least one of a polycarboxylate water reducer, a naphthalene-based water reducer, a lignin sulfonate water reducer, and the like.

[0016] Furthermore, the polymer powder includes at least one of polyvinyl alcohol powder (PVA), vinyl acetate and ethylene copolymer powder (Vac / E), ethylene and vinyl chloride and vinyl silicate terpolymer powder (E / Vc / VL), acrylate and styrene copolymer powder (A / S), etc. The polymer powder helps to improve the water resistance of the anchoring agent.

[0017] Furthermore, the resin curing agent includes at least one of aliphatic diamines and polyamines, aromatic polyamines, phthalic anhydride, acid anhydride, methyl ethyl ketone peroxide, cyclohexanone peroxide, methyl isobutyl ketone peroxide, and the like.

[0018] Furthermore, the phosphate includes at least one of ammonium dihydrogen phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, etc.

[0019] Furthermore, the retarder includes at least one of borax, boric acid, triethanolamine and the like.

[0020] Furthermore, the mineral admixture includes at least one of fly ash, metakaolin, silica fume, slag, modified coal slime, etc. Optionally, the fineness of the mineral admixture is 400-600 mesh.

[0021] The modified coal slime is prepared by the following method: the coal slime is mixed with a calcination dispersant and then calcined, and then the calcined product is ground and an activator is added to obtain the modified coal slime.

[0022] Furthermore, the calcination dispersant is 2-5% of the mass of the coal slime. Optionally, the calcination dispersant includes at least one of magnesium aluminate powder, magnesium silicate powder, calcium silicate powder, etc. The calcination dispersant can be adsorbed on the surface of the coal slime to increase its surface area and ensure its stability in subsequent processes.

[0023] Furthermore, the calcination temperature is 700-850°C and the time is 24-36 hours. Calcination can effectively remove weak components such as carbon on the surface and inside of the coal slime and form a dense structure, thereby improving the strength and activity of the coal slime.

[0024] Further, the activator is 3-6% of the mass of the calcined product. Optionally, the activator includes at least one of sodium hydroxide solution, potassium hydroxide solution, phosphoric acid, etc. Optionally, the mass fraction of the sodium hydroxide solution, potassium hydroxide solution, and phosphoric acid is 15-25%.

[0025] Secondly, the present invention provides a method for using the resin-modified dual-speed magnesium phosphate cement anchor, comprising the following steps:

[0026] (1) First, the A component and the B component of the fast-setting slurry stored separately are placed in the top space of the anchor hole where the anchor rod is installed. Then, the A component and the B component of the slow-setting slurry stored separately are placed in the bottom space of the anchor hole.

[0027] (2) Insert the anchor rod into the anchor hole and rotate the anchor rod to mix the slurries evenly. Then apply prestress to the anchor rod, and wait for the slurry to solidify.

[0028] Furthermore, in step (1), the slurry may be placed in a membrane bag, a glass tube, or injected into a predetermined position of the anchor hole.

[0029] Compared with the prior art, the present invention has at least the following beneficial technical effects:

[0030] (1) The magnesium phosphate cement anchor of the present invention has the characteristics of double-speed setting and full-length anchoring. This is because: after the fast-setting slurry enters the anchor hole, it quickly solidifies to achieve the initial anchor force and forms the first bearing layer. After the preload force is applied, the slow-setting slurry gradually solidifies to form the second bearing layer, and finally realizes the multi-layer thickened bearing arch pressure bearing. At this time, the applied preload force has acted on the solidified anchor body, forming a constraint body of equal density and strength with the surrounding surrounding rock. Even if the anchor rod breaks, the efficiency of the bearing arch of the entire surrounding rock will not change. It not only solves the harm of water spraying to the anchoring strength, but also realizes the multi-layer thickened bearing arch pressure bearing under special conditions such as broken zones, faults, impact pressure, high stress concentration and soft rock crushing, which can achieve the top plate preventable and controllable, safe and reliable tunnel and efficient operation.

[0031] (2) After the A component and the B component are mixed, the heavy-burned magnesium oxide and the phosphate form magnesium phosphate cement, which undergoes a hydration reaction under the action of water to form a hydration product with high strength and high adhesion. At the same time, the unsaturated polyester resin wets the surface of the magnesium phosphate cement and penetrates into the microporous structure of the hydration product of the magnesium phosphate cement; however, the present invention finds that the surface tension of the unsaturated polyester resin is different from that of the magnesium phosphate cement, resulting in an interface region between the high modulus magnesium phosphate cement and the low modulus resin, which leads to insufficient interface bonding strength and poor stability between the two, and easily generates stress concentration at the interface, thereby causing interface damage or delamination. In addition, the existence of the interface region directly affects the ability to withstand alternating loads and reduces the overall mechanical properties of the material. To this end, the present invention modifies the unsaturated polyester resin by using nano-SiO2 and a silane coupling agent. Wherein: the hydrolyzable functional group (alkoxy, etc.) in the silane coupling agent reacts with the hydroxyl or carboxyl group in the unsaturated polyester resin, which not only enhances the interface bonding force between the resin and the nano-SiO2, but also can "tighten" the unsaturated polyester resin on the interface through the SiO2. Thus, the modulus of the interface zone is between the inorganic reinforcement material and the resin, and the stress of the anchoring agent can be uniformly transmitted. At the same time, the silane coupling agent increases the surface tension of the nano-SiO2, which is conducive to the infiltration and expansion of the resin on the inorganic surface, improves the wetting ability of the resin to the inorganic reinforcement material, and makes the resin and the inorganic reinforcement material bonded together better. In addition, the dispersibility and compatibility of the nano-SiO2 in the resin are also significantly improved.

[0032] (3) The modified unsaturated polyester resin of the present invention can generate free radicals under the action of the accelerator and the resin curing agent, and the molecular chain grows rapidly to form a three-way cross-linked macromolecular network, and then reacts with the hydration product of magnesium phosphate cement to form a three-dimensional network cross-linked structure, which can firmly bond the anchor rod to the surrounding rock. At the same time, since magnesium phosphate cement releases a large amount of heat when solidifying, the temperature of the system is increased, so that the generation of free radicals and the copolymerization and cross-linking reaction of the unsaturated double bonds on the main chain of the unsaturated polyester resin are more rapid, and the unsaturated double bonds on the main chain of the unsaturated polyester resin can participate in the polymerization reaction more fully, thereby improving the curing degree and curing speed between the magnesium phosphate cement and the resin. At the same time, the magnesium phosphate cement and the unsaturated polyester resin react to form a three-dimensional network cross-linked structure, which improves the overall water resistance of the anchor body, so that the strength can also develop normally in a water-containing environment, meeting the anchoring requirements of the seepage area and the water sprinkling area. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein:

[0034] Figure 1 This is a sample picture of the fast-setting slurry prepared in Example 1 below.

[0035] Figure 2 This is a sample picture of the slow setting slurry prepared in Example 1 below. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.

[0037] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention.

[0038] Example 1

[0039] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchor comprises the following steps:

[0040] 1. Preparation of rapid setting slurry:

[0041] (1) Take 20 parts by weight of 196 type unsaturated polyester resin, 0.1 parts by weight of benzoyl peroxide, 0.05 parts by weight of dimethylaniline, 1.2 parts by weight of silane coupling agent (KH550), and 5 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 70°C, and stir them continuously at this temperature for 180 minutes to obtain modified unsaturated polyester resin.

[0042] (2) Preparation of component A: 30 parts by weight of the modified unsaturated polyester resin prepared in this example, 45 parts by weight of dead-burned magnesium oxide powder, 30 parts by weight of 500-mesh fly ash, 3 parts by weight of 10 mm-long polyvinyl alcohol fiber, 1.5 parts by weight of polycarboxylic acid water-reducing agent, 80 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 5 parts by weight of polyvinyl alcohol rubber powder, and 20 parts by weight of water are mixed and stirred evenly to obtain component A.

[0043] (3) Preparation of component B: Take 2.5 parts by weight of resin curing agent (methyl ethyl ketone peroxide), 40 parts by weight of ammonium dihydrogen phosphate, 0.5 parts by weight of borax, and 6.5 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix it with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry, such as Figure 1 shown.

[0044] 2. Preparation of slow-setting slurry:

[0045] (i) Take 20 parts by weight of 196 type unsaturated polyester resin, 0.05 parts by weight of benzoyl peroxide, 0.05 parts by weight of dimethylaniline, 1.2 parts by weight of silane coupling agent (KH550), and 1 part by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 70°C, and stir them continuously at this temperature for 180 minutes to obtain a modified unsaturated polyester resin.

[0046] (ii) Preparation of component A: 30 parts by weight of the modified unsaturated polyester resin prepared in this example, 45 parts by weight of dead-burned magnesium oxide powder, 30 parts by weight of 500-mesh fly ash, 3 parts by weight of 10 mm-long polyvinyl alcohol fiber, 1.5 parts by weight of polycarboxylic acid water-reducing agent, 80 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 5 parts by weight of polyvinyl alcohol rubber powder, and 20 parts by weight of water were mixed and stirred evenly to obtain component A.

[0047] (iii) Preparation of component B: Take 2.5 parts by weight of resin curing agent (methyl ethyl ketone peroxide), 40 parts by weight of ammonium dihydrogen phosphate, 1.5 parts by weight of borax, and 6.5 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix it with the component A prepared in step (ii) and stir them evenly to obtain a slow-setting slurry, such as Figure 2 shown.

[0048] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0049] .

[0050] Example 2

[0051] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchor comprises the following steps:

[0052] 1. Preparation of rapid setting slurry:

[0053] (1) Take 135 parts by weight of 196 type unsaturated polyester resin, 1.5 parts by weight of ethylenediamine, 2 parts by weight of dimethylaniline, 2 parts by weight of silane coupling agent (KH570), and 8 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 50°C, and stir them continuously at this temperature for 300 minutes to obtain modified unsaturated polyester resin.

[0054] (2) Preparation of Component A: 135 parts by weight of the modified unsaturated polyester resin prepared in this example, 90 parts by weight of dead-burned magnesium oxide powder, 50 parts by weight of 600-mesh silica fume, 5 parts by weight of 3 mm-long basalt fiber, 3 parts by weight of polycarboxylic acid water-reducing agent, 135 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 10 parts by weight of vinyl acetate and ethylene copolymer rubber powder, and 25 parts by weight of water. Mix the above raw materials and stir evenly to obtain Component A.

[0055] (3) Preparation of component B: Take 4 parts by weight of resin curing agent (methyl isobutyl ketone peroxide), 45 parts by weight of ammonium dihydrogen phosphate, 1.5 parts by weight of boric acid, and 8 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the above raw materials with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0056] 2. Preparation of slow-setting slurry:

[0057] (i) Take 135 parts by weight of 196 type unsaturated polyester resin, 0.5 parts by weight of ethylenediamine, 2 parts by weight of dimethylaniline, 2 parts by weight of silane coupling agent (KH570), and 8 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 50°C, and stir them continuously at this temperature for 300 minutes to obtain modified unsaturated polyester resin.

[0058] (ii) Preparation of component A: 135 parts by weight of the modified unsaturated polyester resin prepared in this example, 90 parts by weight of dead-burned magnesium oxide powder, 50 parts by weight of 600-mesh silica fume, 5 parts by weight of basalt fiber with a length of 3 mm, 3 parts by weight of polycarboxylic acid water-reducing agent, 135 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 10 parts by weight of vinyl acetate and ethylene copolymer rubber powder, and 25 parts by weight of water are mixed and stirred evenly to obtain component A.

[0059] (iii) Preparation of component B: Take 4 parts by weight of resin curing agent (methyl isobutyl ketone peroxide), 45 parts by weight of ammonium dihydrogen phosphate, 3 parts by weight of boric acid, and 8 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0060] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0061] .

[0062] Example 3

[0063] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchor comprises the following steps:

[0064] 1. Preparation of rapid setting slurry:

[0065] (1) Take 10 parts by weight of 196 type unsaturated polyester resin, 0.02 parts by weight of triethanolamine, 0.1 parts by weight of dimethylaniline, 0.1 parts by weight of silane coupling agent (KH792), and 1 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 80°C, and stir them continuously at this temperature for 100 minutes to obtain modified unsaturated polyester resin.

[0066] (2) Preparation of modified coal slime: Coal slime was mixed with magnesium aluminate powder (magnesium aluminate powder was 5% of the mass of coal slime) and stirred, and then heated to 850°C at a heating rate of 10°C / min and calcined for 24 hours. Then it was cooled to room temperature, the calcined product was ground and passed through a 400-mesh sieve, and then 15% sodium hydroxide solution was added and stirred evenly (the sodium hydroxide solution was 6% of the mass of the calcined product), and the modified coal slime was obtained.

[0067] (3) Preparation of Component A: 10 parts by weight of the modified unsaturated polyester resin prepared in this example, 30 parts by weight of dead-burned magnesium oxide powder, 10 parts by weight of the modified coal slime prepared in this example, 1 part by weight of polypropylene fiber with a length of 12 mm, 1.5 parts by weight of sodium lignosulfonate water reducer, 50 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 1 part by weight of acrylic acid ester and styrene copolymer rubber powder, and 10 parts by weight of water. Mix the above raw materials and stir evenly to obtain Component A.

[0068] (4) Preparation of component B: Take 0.2 parts by weight of resin curing agent (cyclohexanone peroxide), 18 parts by weight of potassium dihydrogen phosphate, 0.5 parts by weight of boric acid, and 5 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0069] 2. Preparation of slow-setting slurry:

[0070] (1) Take 10 parts by weight of 196 type unsaturated polyester resin, 0.01 parts by weight of triethanolamine, 0.1 parts by weight of dimethylaniline, 0.1 parts by weight of silane coupling agent (KH792), and 1 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 80°C, and stir them continuously at this temperature for 100 minutes to obtain modified unsaturated polyester resin.

[0071] (2) Preparation of modified coal slime: Coal slime was mixed with magnesium silicate powder (magnesium silicate powder was 4% of the mass of coal slime) and stirred, and then heated to 850°C at a heating rate of 10°C / min and calcined for 24 hours. Then it was cooled to room temperature, the calcined product was ground and passed through a 400-mesh sieve, and then 20% potassium hydroxide solution was added and stirred evenly (the potassium hydroxide solution was 5% of the mass of the calcined product), and the modified coal slime was obtained.

[0072] (3) Preparation of Component A: 10 parts by weight of the modified unsaturated polyester resin prepared in this example, 30 parts by weight of dead-burned magnesium oxide powder, 10 parts by weight of the modified coal slime prepared in this example, 1 part by weight of polypropylene fiber with a length of 12 mm, 1.5 parts by weight of sodium lignosulfonate water reducer, 50 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 1 part by weight of acrylic acid ester and styrene copolymer rubber powder, and 10 parts by weight of water. Mix the above raw materials and stir evenly to obtain Component A.

[0073] (4) Preparation of component B: Take 0.2 parts by weight of resin curing agent (cyclohexanone peroxide), 18 parts by weight of potassium dihydrogen phosphate, 2 parts by weight of boric acid, and 5 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0074] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0075] .

[0076] Example 4

[0077] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchor comprises the following steps:

[0078] 1. Preparation of rapid setting slurry:

[0079] (1) Take 80 parts by weight of 196 type unsaturated polyester resin, 1 part by weight of cyclohexanone peroxide, 0.7 parts by weight of dimethylaniline, 1.2 parts by weight of silane coupling agent (DL602), and 4 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 60°C, and stir them continuously at this temperature for 250 minutes to obtain modified unsaturated polyester resin.

[0080] (2) Preparation of modified coal slime: Coal slime was mixed with calcium silicate powder (calcium silicate powder was 2% of the mass of coal slime) and stirred, and then heated to 700°C at a heating rate of 10°C / min and calcined for 36 hours. Then it was cooled to room temperature, the calcined product was ground and passed through a 400-mesh sieve, and then 25% by mass phosphoric acid was added and stirred evenly (the phosphoric acid was 3% by mass of the calcined product), and the modified coal slime was obtained.

[0081] (3) Preparation of Component A: 70 parts by weight of the modified unsaturated polyester resin prepared in this example, 50 parts by weight of dead-burned magnesium oxide powder, 25 parts by weight of the modified coal slime prepared in this example, 3 parts by weight of glass fiber with a length of 5 mm, 2 parts by weight of sodium wood sulfonate water reducer, 90 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 6 parts by weight of ethylene, vinyl chloride and vinyl silicate ternary copolymer rubber powder, and 20 parts by weight of water. Mix the above raw materials and stir evenly to obtain Component A.

[0082] (4) Preparation of component B: Take 1.5 parts by weight of resin curing agent (cyclohexanone peroxide), 35 parts by weight of sodium dihydrogen phosphate, and 7 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0083] (3) Preparation of component B: Take 1.5 parts by weight of resin curing agent (cyclohexanone peroxide), 35 parts by weight of sodium dihydrogen phosphate, and 7 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0084] 2. Preparation of slow-setting slurry:

[0085] (1) Take 80 parts by weight of unsaturated polyester resin powder, 0.25 parts by weight of cyclohexanone peroxide, 0.7 parts by weight of dimethylaniline, 1.2 parts by weight of silane coupling agent (DL602), and 4 parts by weight of nano-SiO2. Mix the above raw materials evenly, heat them in a water bath to 60°C, and stir them continuously at this temperature for 250 minutes to obtain modified unsaturated polyester resin.

[0086] (2) Preparation of modified coal slime: Coal slime was mixed with calcium silicate powder (calcium silicate powder was 3% of the mass of coal slime) and stirred, and then heated to 700°C at a heating rate of 10°C / min and calcined for 36 hours. Then it was cooled to room temperature, the calcined product was ground and passed through a 400-mesh sieve, and then 25% by mass phosphoric acid was added and stirred evenly (the phosphoric acid was 3% by mass of the calcined product), and the modified coal slime was obtained.

[0087] (3) Preparation of Component A: 70 parts by weight of the modified unsaturated polyester resin prepared in this example, 50 parts by weight of dead-burned magnesium oxide powder, 25 parts by weight of the modified coal slime prepared in this example, 3 parts by weight of glass fiber with a length of 5 mm, 2 parts by weight of sodium wood sulfonate water reducer, 90 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 6 parts by weight of ethylene, vinyl chloride and vinyl silicate ternary copolymer rubber powder, and 20 parts by weight of water. Mix the above raw materials and stir evenly to obtain Component A.

[0088] (4) Preparation of component B: Take 1.5 parts by weight of resin curing agent (cyclohexanone peroxide), 35 parts by weight of sodium dihydrogen phosphate, 1.2 parts by weight of triethanolamine, and 7 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0089] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0090] .

[0091] Example 5

[0092] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchor comprises the following steps:

[0093] 1. Preparation of rapid setting slurry:

[0094] (1) Preparation of component A: 30 parts by weight of 196 type unsaturated polyester resin, 45 parts by weight of dead-burned magnesium oxide powder, 30 parts by weight of 500-mesh fly ash, 3 parts by weight of 10 mm long polyvinyl alcohol fiber, 1.5 parts by weight of polycarboxylic acid water reducer, 80 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 5 parts by weight of polyvinyl alcohol rubber powder, and 20 parts by weight of water. Mix the above raw materials and stir evenly to obtain component A.

[0095] (2) Preparation of component B: Take 2.5 parts by weight of resin curing agent (methyl ethyl ketone peroxide), 40 parts by weight of ammonium dihydrogen phosphate, 0.5 parts by weight of borax, and 6.5 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the component B with the component A prepared in step (2) and stir them evenly to obtain a quick-setting slurry.

[0096] 2. Preparation of slow-setting slurry:

[0097] (i) Preparation of component A: 30 parts by weight of 196 type unsaturated polyester resin, 45 parts by weight of dead-burned magnesium oxide powder, 30 parts by weight of 500-mesh fly ash, 3 parts by weight of 10 mm-long polyvinyl alcohol fiber, 1.5 parts by weight of polycarboxylic acid water reducer, 80 parts by weight of river sand fine aggregate with a particle size of 0.2-0.5 mm, 5 parts by weight of polyvinyl alcohol rubber powder, and 20 parts by weight of water. Mix the above raw materials and stir evenly to obtain component A.

[0098] (ii) Preparation of component B: Take 2.5 parts by weight of resin curing agent (methyl ethyl ketone peroxide), 40 parts by weight of ammonium dihydrogen phosphate, 1.5 parts by weight of borax, and 6.5 parts by weight of water. Mix the above raw materials and stir them evenly to obtain component B. Mix the above raw materials with the component A prepared in step (ii) and stir them evenly to obtain a slow-setting slurry.

[0099] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0100] .

[0101] Example 6

[0102] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchoring agent is different from the above-mentioned Example 2 in that no silane coupling agent is added in the preparation of the fast-setting slurry and the slow-setting slurry of this example.

[0103] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0104] .

[0105] Example 7

[0106] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchoring agent is different from the above-mentioned Example 2 in that nano-SiO2 is not added in the preparation of the fast-setting slurry and the slow-setting slurry of this example.

[0107] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0108] .

[0109] Example 8

[0110] A method for preparing a resin-modified dual-speed magnesium phosphate cement anchoring agent is different from the above-mentioned Example 3 in that no accelerator is added in the preparation of the fast-setting slurry and the slow-setting slurry in this example.

[0111] According to "Resin Anchor Part 1: Anchoring Agent" (MT146.1-2011), the setting time and compressive strength of the fast-setting slurry and slow-setting slurry prepared in this embodiment were tested respectively, and the results are shown in the following table:

[0112] .

[0113] From the test results of the above embodiments, it can be seen that the various performance indicators of the magnesium phosphate cement anchor prepared by embodiments 1 to 4 of the technical solution proposed by the present invention are significantly better than those of the comparative solution (embodiments 5 to 8), which shows that the magnesium phosphate cement anchor prepared by the technical solution proposed by the present invention has better strength and thus has stronger anchoring force. At the same time, the magnesium phosphate cement anchor prepared by the technical solution proposed by the present invention can better develop strength in a water-containing environment, thereby better meeting the anchoring requirements of the seepage area and the water sprinkling area.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still repair the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any repair, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A resin-modified dual-speed magnesium phosphate cement anchor, characterized in that: include: The mass ratio of the fast-setting slurry and the slow-setting slurry is 0.5-1:1; both slurries include component A and component B: The component A comprises: 10-135 parts by weight of modified unsaturated polyester resin, 30-90 parts by weight of dead-burned magnesium oxide powder, 10-50 parts by weight of mineral admixture, 1-5 parts by weight of fiber, 1.5-3 parts by weight of water reducer, 50-135 parts by weight of fine aggregate, 1-10 parts by weight of polymer rubber powder, and 10-25 parts by weight of water; The B component includes: 0.2-4 parts by weight of resin curing agent, 18-45 parts by weight of phosphate, 0-3 parts by weight of retarder, and 5-8 parts by weight of water, and the amount of retarder in the fast-setting slurry is 25-50% of the amount of retarder in the slow-setting slurry; and the retarder in the slow-setting slurry is not less than 1.2 parts by weight; The modified unsaturated polyester resin is prepared by the following method: unsaturated polyester resin, accelerator, dimethylaniline, silane coupling agent and nano-SiO2 are mixed and heated and stirred to obtain the modified unsaturated polyester resin; the amount of the accelerator of the modified unsaturated polyester resin in the slow-setting slurry is 25-50% of the amount of the accelerator in the fast-setting slurry; The ratio of the unsaturated polyester resin, accelerator, dimethylaniline, silane coupling agent and nano-SiO2 is 10-135 parts by weight: 0.01-1.5 parts by weight: 0.1-2 parts by weight: 0.1-2 parts by weight: 1-8 parts by weight; The accelerator comprises at least one of benzoyl peroxide, cyclohexanone peroxide, formic acid, ethylenediamine and triethanolamine.

2. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The silane coupling agent includes at least one of KH550, KH560, KH570, KH792, and DL602.

3. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The heating and stirring is performed at a temperature of 50-80° C. and for a time of 100-300 min.

4. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The fiber comprises: at least one of basalt fiber, polyvinyl alcohol fiber, steel fiber, carbon fiber, glass fiber and polypropylene fiber.

5. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The length of the fiber is 3 to 12 mm.

6. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The water reducer comprises at least one of a polycarboxylate water reducer, a naphthalene-based water reducer and a lignin sulfonate water reducer.

7. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The polymer rubber powder comprises at least one of polyvinyl alcohol rubber powder, vinyl acetate and ethylene copolymer rubber powder, ethylene and vinyl chloride and vinyl silicate ternary copolymer rubber powder, and acrylate and styrene copolymer rubber powder.

8. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The resin curing agent includes at least one of aliphatic diamines and polyamines, aromatic polyamines, phthalic anhydride, acid anhydride, methyl ethyl ketone peroxide, cyclohexanone peroxide, and methyl isobutyl ketone peroxide.

9. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The phosphate includes at least one of ammonium dihydrogen phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate.

10. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 1, characterized in that: The retarder comprises at least one of borax, boric acid and triethanolamine.

11. The resin-modified dual-speed magnesium phosphate cement anchor according to any one of claims 1 to 10, characterized in that: The fineness of the mineral admixture is 400-600 meshes.

12. The resin-modified dual-speed magnesium phosphate cement anchor according to any one of claims 1 to 10, characterized in that: The mineral admixture comprises at least one of fly ash, metakaolin, silica fume, slag and modified coal slime.

13. The resin-modified dual-speed magnesium phosphate cement anchoring agent according to claim 12, characterized in that: The modified coal slime is prepared by the following method: the coal slime is mixed with a calcination dispersant and then calcined, and then the calcined product is ground and an activator is added to obtain the modified coal slime.

14. The resin-modified dual-speed magnesium phosphate cement anchoring agent according to claim 13, characterized in that: The calcination dispersant is 2-5% of the mass of the coal slime.

15. The resin-modified dual-speed magnesium phosphate cement anchoring agent according to claim 13, characterized in that: The calcination dispersant comprises at least one of magnesium aluminate powder, magnesium silicate powder and calcium silicate powder.

16. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 13, characterized in that: The calcination temperature is 700-850° C. and the calcination time is 24-36 hours.

17. The resin-modified dual-speed magnesium phosphate cement anchor according to claim 13, characterized in that: The activator is 3-6% of the mass of the calcined product.

18. The resin-modified dual-speed magnesium phosphate cement anchoring agent according to claim 13, characterized in that: The activator includes at least one of sodium hydroxide solution, potassium hydroxide solution and phosphoric acid.

19. The resin-modified dual-speed magnesium phosphate cement anchoring agent according to claim 18, characterized in that: The mass fraction of the sodium hydroxide solution, potassium hydroxide solution and phosphoric acid is 15-25%.

20. The method for using the resin-modified dual-speed magnesium phosphate cement anchoring agent according to any one of claims 1 to 19, characterized in that: The steps include: (1) firstly, placing the A component and the B component of the fast-setting slurry stored separately into the top space of the anchor hole in which the anchor rod is installed; then, placing the A component and the B component of the slow-setting slurry stored separately into the bottom space of the anchor hole; (2) Insert the anchor rod into the anchor hole and rotate the anchor rod to mix the slurries evenly; then apply prestress to the anchor rod, and wait for the slurry to solidify.