A method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid
By mixing lithium mica with spodumene concentrate for high-temperature roasting and low-temperature sulfuric acid calcination, combined with water-immersed solid-liquid separation, the problems of high smelting slag volume and insufficient lithium leaching rate in lithium mica lithium extraction were solved, and high efficiency and low Cost lithium extraction, suitable for industrial applications.
Patent Information
- Application Number
- CN202410742798.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Among the existing lithium mica lithium extraction methods, the sulfate method has the problems of high sludge volume, high cost, high sodium and potassium concentration, easy to knead ring and lithium leaching rate of less than 90%. It is urgent to develop economically feasible, easy to practice and Technology with high lithium recovery rate.
将锂云母精矿与锂辉石精矿均匀混合进行高温焙烧,随后与硫酸均匀混合进行低温煅烧,最后在水中进行水浸固液分离,得到锂浸出液和浸锂尾渣,利用高温焙烧和低温 Sulfuric acid calcination works synergistically to significantly improve the lithium extraction efficiency.
Significantly reduce the amount of smelting slag, increase the lithium leaching rate, reduce energy consumption and cost, avoid baking sintering rings, simplify the process flow, is suitable for industrial applications, and improve the comprehensive utilization rate of lithium resources.
Smart Images

Figure CN118639032B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium extraction from lithium ore, and in particular to a method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid. Background Art
[0002] As "white oil", lithium is closely related to the development of my country's new energy emerging industries. my country is a country with very rich lithium resources, but its external dependence is very high. Lepidolite is a relatively abundant hard rock lithium mineral resource in my country, with a chemical composition of K{Li (2-x) Al (1+x) [Al 2x Si (4-2x) O 10 ](OH,F)2}(x=0-0.5), the content of Li2O is generally around 4wt%. With the rapid development of our new energy industry, the demand for lithium is increasing day by day. The efficient development and utilization of this resource is of great significance to the development of my country's lithium industry and emerging industries.
[0003] Lepidolite is a lithium-containing aluminum silicate that exists in the form of a complex aggregate of fine flakes. Extracting lithium from it is a complex chemical process. The relevant extraction technology has been developing in the direction of comprehensive resource utilization, reducing pollutant emissions, and simplifying process flow. At present, the methods for extracting lithium from lepidolite include sulfate method, sulfuric acid method, high-pressure alkali boiling method, chloride method, and mechanical activation. Among them, the sulfate method and sulfuric acid method have industrial application cases, and the former is more widely used, but these two methods also have some problems that need to be solved. Patents CN117776231A and CN116445736A disclose two methods for extracting lithium from lithium mica using composite sulfates, but the proportion of composite salts is too high (greater than 50%, up to 300%), the cost is high, and the high proportion of additives causes the amount of smelting slag to be much higher than the quality of the raw materials of lithium ore entering the smelting. According to statistics, using the sulfate method to process lithium mica, for every ton of lithium carbonate produced, about 15 to 21 tons of smelting slag are produced, and the quality of smelting slag is significantly higher than the quality of lithium mica concentrate entering the smelting, and the disposal cost of smelting slag is high; in addition, because sulfate introduces a large amount of sodium and potassium, the concentration of sodium and potassium in the leachate is high, which brings certain obstacles to the subsequent purification process. In addition, various manufacturers in the industry have also pointed out that the sulfate method has the dilemma of easy ring formation during roasting and the lithium leaching rate is less than 90%. Patent CN106755967A proposes a method for treating lithium mica with sulfuric acid roasting and preparing lithium carbonate, but this method has the problems of large amount of sulfuric acid residue and high amount of Al dissolution. A large amount of Al(OH)3 colloid is produced in the purification stage, which will adsorb lithium in the solution and reduce the lithium extraction rate. Obviously, it is urgent to develop a lithium extraction technology for lithium mica that is economically feasible, easy to practice, and has a high lithium recovery rate. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for efficiently extracting lithium by calcining spodumene lepidolite with sulfuric acid at low temperature. The method comprises the following steps: first, uniformly mixing lepidolite concentrate with spodumene concentrate and then performing high-temperature roasting to obtain a roasting material; then, uniformly mixing the roasting material with sulfuric acid and performing low-temperature calcining to obtain an acidified material; finally, placing the acidified material in water for water leaching, and then performing solid-liquid separation to obtain a lithium leaching solution and lithium leaching tailings; the method significantly improves the efficiency of lithium extraction from hard rock lithium ore; the lithium leaching rate is extremely high, while the leaching rates of impurity elements such as aluminum, sodium and potassium are low; the amount of smelting slag produced by the method for producing 1 ton of lithium carbonate product is reduced by about 50% compared with the traditional sulfate method; the technical solution has simple process, low energy consumption and low cost, is suitable for industrial application, plays an extremely important role in the efficient development and utilization of lithium resources, and has excellent application and promotion prospects.
[0005] In order to achieve the above technical effects, the following technical solutions are adopted:
[0006] A method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid comprises the following steps:
[0007] Step S1: uniformly mixing the lepidolite concentrate and the spodumene concentrate and then calcining them at high temperature to obtain a calcined material;
[0008] Step S2: uniformly mixing the roasted material in step S1 with sulfuric acid, and calcining at low temperature to obtain an acidified material;
[0009] Step S3: placing the acidified material in step S2 in water for water leaching, and then performing solid-liquid separation to obtain lithium leaching solution and lithium leaching tailings, wherein the lithium extraction rate in the leaching solution is greater than 97%.
[0010] Furthermore, the lepidolite concentrate is one or both of ferrolithium mica and lepidolite.
[0011] Furthermore, the lithium content of the lepidolite concentrate is 0.3-2.0wt%; the lithium content of the spodumene concentrate is 1.5-3.7wt%.
[0012] Furthermore, the mixing mass ratio of the lepidolite concentrate and the spodumene concentrate is 0.1:1 to 3.0:1.
[0013] Too little or too much lithium mica dosage is not conducive to the synergistic transformation of the mineral phases of lithium mica and spodumene and the synergistic lithium extraction effect with the subsequent low-temperature calcination of sulfuric acid.
[0014] Furthermore, the high temperature calcination temperature in step S1 is 800-950°C.
[0015] Controlling the roasting reaction temperature and time within a reasonable range is conducive to improving the roasting efficiency. When the roasting temperature is too low or the time is too short, the mineral phase synergistic transformation of lepidolite and spodumene cannot be completed. When the roasting temperature is too high or the time is too long, the roasting energy consumption will increase.
[0016] Furthermore, the high temperature roasting time in step S1 is 30 to 90 minutes.
[0017] Furthermore, in step S2, the amount of sulfuric acid mixed with the calcined material is 1.2 to 1.5 times the theoretical acid consumption when all the lithium elements in the spodumene lepidolite concentrate are converted into lithium sulfate, and the sulfuric acid is concentrated sulfuric acid.
[0018] If the amount of sulfuric acid used is too low, the lithium replacement cannot be completely completed and the lithium leaching rate is low; if the amount of sulfuric acid used is too high, the content of impurity elements in the lithium extraction leaching solution will increase, the equipment will corrode seriously, and it will not be economical.
[0019] Furthermore, the temperature of the low-temperature calcination in step S2 is 150-300°C.
[0020] Furthermore, the low-temperature calcination time in step S2 is 10 to 60 minutes.
[0021] Controlling the calcination reaction temperature and time within a reasonable range is conducive to improving the efficiency of ion cooperative replacement. Calcination temperature that is too low or time that is too short will lead to insufficient lithium replacement rate, while calcination temperature that is too high or time that is too long will increase calcination energy consumption.
[0022] Furthermore, the water immersion reaction conditions in step S3 are: liquid-solid ratio of 2-8 mL:1 g, temperature of 20-80° C., and time of 30-90 min.
[0023] Controlling the liquid-to-solid ratio, leaching temperature and leaching time in the water leaching process within a reasonable range can improve the leaching efficiency and help obtain a lithium extraction solution with higher purity. A too low liquid-to-solid ratio, too low leaching temperature or too short leaching time will relatively reduce the lithium extraction rate; while a too high liquid-to-solid ratio will result in too low lithium concentration in the leaching solution, which is not conducive to subsequent evaporation and concentration; too high leaching temperature or too long time will increase leaching energy consumption.
[0024] The beneficial effects of the present invention are:
[0025] (1) Low smelting slag volume. The traditional lithium mica sulfate method produces 15 to 21 tons of lithium mica smelting slag for every ton of lithium carbonate produced. This technical solution only produces 7 to 11 tons of smelting slag for every ton of lithium carbonate produced, reducing the slag volume by more than half, which is conducive to the industrial consumption of smelting slag.
[0026] (2) The comprehensive utilization rate of lithium resources is high, and the energy consumption of roasting is low. The traditional lithium extraction process of spodumene sulfuric acid requires a high-temperature roasting transformation process of more than 1050°C. The sulfate or sulfuric acid method of lithium mica also requires a high-temperature roasting of more than 900°C. However, the temperature of the mineral phase synergistic transformation of lithium mica and spodumene mixture only needs 800-950°C. Combined with the subsequent low-temperature calcination of sulfuric acid, the mineral phase transformation and the low-temperature calcination of sulfuric acid to disintegrate the minerals synergistically enhance the efficiency of lithium extraction, greatly improving the efficiency of lithium extraction. The lithium extraction rate is generally greater than 95%, which is better than the traditional lithium mica sulfate method and sulfuric acid method, and is suitable for processing various complex lithium mineral resources.
[0027] (3) The composition of the leachate is relatively simple. Compared with the lithium mica sulfate method, no sulfates such as sodium, potassium, calcium and magnesium need to be added, and the concentrations of sodium and potassium in the leachate are significantly reduced; compared with the lithium mica sulfate method, the aluminum leaching rate is significantly reduced, and the aluminum concentration in the solution is significantly reduced, which alleviates the burden of leachate purification and improves the lithium recovery rate.
[0028] (4) Avoiding serious ring formation during sintering. The mixture of low-melting-point lepidolite and high-melting-point spodumene can alleviate the ring formation problem in the rotary kiln during high-temperature sintering, which is beneficial to continuous production in industry.
[0029] (5) The method is simple, the conditions are mild, the cost is low, and the process is highly adaptable. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. The drawings in the following description are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0031] Figure 1 It is a process schematic diagram of a method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0033] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0034] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.
[0035] Embodiment 1:
[0036] according to Figure 1 As shown, the lithium extraction operation of lithium ore is carried out:
[0037] Take 50g of lithium mica concentrate with a Li content of 1.25wt.% and 50g of spodumene concentrate with a Li content of 2.98wt.%, mix them evenly, and then place them in a muffle furnace for high-temperature roasting, the roasting temperature is set to 800℃, and the roasting time is 90min. After the roasting material is cooled to 100℃, it is ball-milled to less than 100 mesh, and then concentrated sulfuric acid is added according to 1.5 times of the theoretical acid consumption and evenly mixed. The mixed acid material is placed in a muffle furnace for low-temperature calcination, the calcination temperature is set to 150℃, and the calcination time is 60min to obtain an acidified material. Subsequently, the acidified material is placed in water for water immersion according to a liquid-to-solid ratio of 4mL:1g, and the leaching temperature is set to 20℃ for 30min. After leaching, it is filtered to obtain a lithium leaching solution and lithium leaching tailings.
[0038] After testing and analysis, the leaching rate of Li in the leaching solution obtained in Example 1 is 97.38%, the leaching rate of Al is 7.00%, the concentrations of Na and K are 0.75 and 0.49 g / L respectively, and the mass of smelting slag is 91.58% (91.58 g) of the mass of lithium ore entering the leaching solution. If the lithium recovery rate of the leaching solution in the process of preparing lithium carbonate is set to 95.00%, it can be converted into 8.79 tons of smelting slag for every ton of lithium carbonate produced. It shows that the technical solution can extract lithium from the mixed concentrate of lepidolite and spodumene at a relatively low energy consumption (850°C), can achieve an ideal lithium extraction rate, effectively control the leaching rate of aluminum, the concentrations of sodium and potassium in the solution are also very low, and can significantly reduce the amount of smelting slag.
[0039] Embodiment 2:
[0040] according to Figure 1 As shown, the lithium extraction operation of lithium ore is carried out:
[0041] Take 50g of lithium mica concentrate with a Li content of 1.25wt.% and 50g of spodumene concentrate with a Li content of 2.98wt.%, mix them evenly, and then place them in a muffle furnace for high-temperature roasting, the roasting temperature is set to 950℃, and the roasting time is 30min. After the roasting material is cooled to 100℃, it is ball-milled to less than 100 mesh, and then concentrated sulfuric acid is added according to 1.2 times of the theoretical acid consumption and evenly mixed. The mixed acid material is placed in a muffle furnace for low-temperature calcination, the calcination temperature is set to 300℃, and the calcination time is 10min to obtain an acidified material. Subsequently, the acidified material is placed in water for water immersion according to a liquid-to-solid ratio of 8mL:1g, and the leaching temperature is set to 80℃ for 90min. After leaching, it is filtered to obtain a lithium leaching solution and lithium leaching tailings.
[0042] After testing and analysis, the leaching rate of Li in the leaching solution obtained in Example 1 is 97.65%, the leaching rate of Al is 7.10%, the concentrations of Na and K are 0.73 and 0.48 g / L respectively, and the mass of smelting slag is 91.48% (91.48 g) of the mass of lithium ore entering the leaching solution. If the lithium recovery rate of the leaching solution in the process of preparing lithium carbonate is set to 95.00%, it can be converted into 8.78 tons of smelting slag for every ton of lithium carbonate produced. It shows that the technical solution can extract lithium from the mixed concentrate of lepidolite and spodumene at a relatively low energy consumption (950°C), can achieve an ideal lithium extraction rate, effectively control the leaching rate of aluminum, the concentrations of sodium and potassium in the solution are also very low, and can significantly reduce the amount of smelting slag.
[0043] Embodiment 3:
[0044] Lithium was extracted by the method of Example 1, except that the mass of spodumene concentrate with a Li content of 2.98 wt.% was 17 g, and the mass of spodumene concentrate with a Li content of 2.98 wt.% was 50 g.
[0045] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the conditions of this embodiment is 96.89%, the leaching rate of Al is 8.25%, the concentrations of Na and K are 0.62 and 0.36 g / L respectively, and the mass of smelting slag is 92.56% (62.01 g) of the mass of lithium ore entering the leaching process. The recovery rate of lithium in the process of preparing lithium carbonate from the leaching solution is set to 95.00%, which can be converted into 11.27 tons of smelting slag for every ton of lithium carbonate produced. Compared with Example 1, the leaching indicators of Example 3 are close, indicating that the ideal lithium leaching effect can also be achieved by appropriately reducing the amount of spodumene.
[0046] Embodiment 4:
[0047] The method of Example 1 is adopted to extract lithium, except that: the Li content is 1.25wt.% lepidolite concentrate is 5g, and the Li content is 2.98wt.% spodumene concentrate is 50g. After detection and analysis, the leaching rate of Li in the obtained leaching solution under the conditions of this embodiment is 95.60%, the leaching rate of Al is 6.50%, the concentrations of Na and K are 0.75 and 0.49g / L respectively, and the quality of smelting slag is 93.77% (51.57g) of the quality of the lithium ore entering the leaching. The recovery rate of lithium in the process of preparing lithium carbonate from the leaching solution is set to 95.00%, which can be converted into 6.92 tons of smelting slag per 1 ton of lithium carbonate produced. Compared with Example 1, the leaching indexes of Example 4 are close, indicating that the desired lithium leaching effect can also be achieved by appropriately reducing the amount of lepidolite.
[0048] Embodiment 5:
[0049] Lithium was extracted by the method of Example 1, except that 50 g of lithium mica concentrate with a Li content of 1.25 wt.% was replaced by 50 g of ferrolithium mica with a Li content of 0.88%.
[0050] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the conditions of this embodiment is 97.23%, the leaching rate of Al is 6.18%, the concentrations of Na and K are 0.23 and 1.07 g / L respectively, and the mass of smelting slag is 93.55% (93.55 g) of the mass of lithium ore entering the leaching solution. The recovery rate of lithium in the process of preparing lithium carbonate from the leaching solution is set to 95.00%, which can be converted into 9.85 tons of smelting slag for every ton of lithium carbonate produced. Compared with Example 1, the leaching indicators of Example 5 are similar, indicating that this method is also suitable for treating iron lithium mica.
[0051] Embodiment 6:
[0052] The method of Example 1 was used to extract lithium, except that the calcination temperature was set at 700°C.
[0053] After testing and analysis, the leaching rate of lithium in the purified solution obtained under the conditions of this embodiment is only 5.34%, the leaching rate of Al is 1.12%, the concentrations of Na and K are 0.11 and 0.06 g / L respectively, and the mass of smelting slag is 98.25% (98.25 g) of the mass of lithium ore leached. Compared with Example 1, the lithium leaching effect of Example 6 is poor, indicating that the temperature of high-multiple roasting needs to be maintained above 800°C.
[0054] Embodiment 7:
[0055] The method of Example 1 was used to extract lithium, except that the amount of sulfuric acid used was 0.75 times the theoretical acid consumption.
[0056] After testing and analysis, the leaching rate of lithium in the purified solution obtained under the conditions of this embodiment is 72.65%, the leaching rate of Al is 4.87%, the concentrations of Na and K are 0.44 and 0.31 g / L respectively, and the mass of smelting slag is 94.66% (94.66 g) of the mass of lithium ore leached. Compared with Example 1, the lithium leaching rate of Example 7 is 24.67 percentage points lower, indicating that the amount of acid used is insufficient to completely complete the replacement of lithium, but the other leaching indicators are similar, indicating that this method still has the advantages of simple leachate composition and low smelting slag amount.
[0057] Embodiment 8:
[0058] The method of Example 1 was used to extract lithium, except that the liquid-to-solid ratio during the water immersion process was set to 2 mL:1 g.
[0059] After testing and analysis, the leaching rate of lithium in the purified solution obtained under the conditions of this embodiment is 96.22%, the leaching rate of Al is 7.89%, the concentrations of Na and K are 1.21 and 0.89 g / L respectively, and the mass of smelting slag is 93.11% (93.11 g) of the mass of lithium ore into leaching. Compared with Example 1, the concentrations of sodium and potassium in the leaching solution of Example 8 are slightly increased, but the other leaching indicators are similar, indicating that appropriately reducing the liquid-to-solid ratio of the leaching process mainly affects the ion concentration in the solution without affecting the leaching effect.
[0060] Comparative Example 1:
[0061] Lithium was extracted by the method of Example 1, except that the Li content was 1.25 wt.%, the lepidolite concentrate was 100 g, and no spodumene concentrate was added.
[0062] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the comparative example conditions is 75.64%, the leaching rate of Al is 72.34%, the concentrations of Na and K are 2.22 and 1.87 g / L respectively, and the mass of smelting slag is 91.58% (91.58 g) of the mass of lithium ore into leaching. Compared with Example 1, the lithium leaching rate of Comparative Example 1 is 21.74 percentage points lower, and the aluminum leaching rate is increased by 65.34 percentage points, indicating that the lithium leaching rate of lithium mica treated by sulfuric acid calcination alone is insufficient, and the leaching rate of impurity element aluminum is significantly higher, which brings certain obstacles to the subsequent purification process.
[0063] Comparative Example 2:
[0064] Lithium is extracted from lepidolite by a composite sulfate method. 50 g of lepidolite concentrate with a Li content of 1.25 wt.% is uniformly mixed with 40% sodium sulfate (20 g), 20% potassium sulfate (10 g) and 20% lime (10 g), and the mixture is roasted at 850° C. for 60 min. After the roasted material is cooled, it is directly leached with water, and the water leaching conditions are consistent with those in Example 1 (liquid-solid ratio is 4 mL:1 g, leaching temperature is 25° C., and leaching time is 30 min). After leaching, the lithium leaching solution and lithium leaching tailings are obtained by filtration.
[0065] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the comparative conditions was 92.12%, the leaching rate of Al was 6.87%, the concentrations of Na and K were 12.31 and 6.28 g / L respectively, and the mass of smelting slag was 121.54% (60.77 g) of the mass of lithium ore entering the leaching solution. Assuming that the recovery rate of lithium in the process of preparing lithium carbonate from the leaching solution is 95.00%, it can be converted into 20.88 tons of smelting slag for every ton of lithium carbonate produced. Compared with Example 1, the lithium leaching rate of Comparative Example 2 is 5.26 percentage points lower, indicating that the lithium leaching effect of lithium mica treated with sulfate method alone is not as good as the method of the technical solution of the present invention (Example 1); the sodium and potassium concentrations in the solution are significantly higher, which will bring huge obstacles to subsequent purification; in addition, the amount of smelting slag is larger, and the amount of slag per ton of product is 1 times higher, which brings great obstacles to the large-scale consumption of smelting slag.
[0066] Comparative Example 3:
[0067] Lithium was extracted by the method of Example 1, except that the Li content was 2.98 wt.%, the spodumene concentrate was 100 g, and no lepidolite concentrate was added.
[0068] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the comparative conditions is 3.37%, the leaching rate of Al is 2.52%, the concentrations of Na and K are 0.08 and 0.09 g / L respectively, and the mass of smelting slag is 97.74% (97.74 g) of the mass of lithium ore leached. Compared with Example 1, the lithium leaching rate of Comparative Example 3 is 94.01 percentage points lower, and the other leaching indicators are similar, indicating that the roasting transformation effect of spodumene treated by sulfuric acid method at 850°C is poor, which is not conducive to the extraction of lithium, which also shows that the technical solution of the present invention (Example 1) has the significant advantage of low energy consumption.
[0069] Comparative Example 4:
[0070] The method of Example 1 was adopted to extract lithium, except that the content of Li was 2.98wt.%, the spodumene concentrate was 100g, and no lepidolite concentrate was added, and the roasted material was cooled and ball-milled without using a sulfuric acid low-temperature calcination process, but directly using sulfuric acid leaching, the amount of sulfuric acid was 5 times the theoretical acid consumption, the sulfuric acid concentration was 4mol / L, the temperature was 90°C, and the stirring was uniform for 90min. After leaching, the lithium leachate and lithium tailings were obtained by filtration.
[0071] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the comparative example conditions was 1.56%, the leaching rate of Al was 2.02%, and the concentrations of Na and K were 0.08 and 0.07 g / L, respectively. Compared with Example 1, the lithium leaching rate of Comparative Example 4 was 95.82 percentage points lower, and the other leaching indicators were similar.
[0072] Comparative Example 5:
[0073] The method of Example 1 was adopted to extract lithium, except that the Li content was 1.25wt.%, the lithium mica concentrate was 100g, and no spodumene concentrate was added, and the roasted material was cooled and ball-milled without using a sulfuric acid low-temperature calcination process, but directly using sulfuric acid leaching, the sulfuric acid dosage was 5 times the theoretical acid consumption, the sulfuric acid concentration was 4mol / L, the temperature was 90°C, and the stirring was uniform for 90min. After leaching, the lithium leachate and lithium leaching tailings were obtained by filtration.
[0074] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the comparative example conditions was 34.42%, the leaching rate of Al was 26.45%, and the concentrations of Na and K were 0.58 and 1.47 g / L, respectively. Compared with Example 1, the lithium leaching rate of Comparative Example 5 was 62.96 percentage points lower, and the other leaching indicators were similar.
[0075] Comparative Example 6:
[0076] The method of Example 1 is used to extract lithium, except that: after the roasted material is cooled and ball-milled, the sulfuric acid low-temperature calcination process is not used, but sulfuric acid is directly used for leaching, the amount of sulfuric acid is 5 times the theoretical acid consumption, the sulfuric acid concentration is 4 mol / L, the temperature is 90°C, and the stirring speed is uniform for 90 minutes. After leaching, the lithium leaching solution and lithium leaching tailings are obtained by filtration.
[0077] After testing and analysis, the leaching rate of Li in the leaching solution obtained under the comparative example conditions was 16.34%, the leaching rate of Al was 13.61%, and the concentrations of Na and K were 0.23 and 1.07 g / L, respectively. Compared with Example 1, the lithium leaching rate of Comparative Example 6 was 81.04 percentage points lower, and the other leaching indicators were similar.
[0078] Comparative Example 1 represents a typical sulfuric acid calcination treatment of lithium mica, Comparative Example 2 represents a sulfate treatment of lithium mica, Comparative Example 3 represents a sulfuric acid calcination treatment of spodumene, Comparative Example 4 represents a high temperature roasting + sulfuric acid leaching treatment of spodumene, Comparative Example 5 represents a high temperature roasting + sulfuric acid leaching treatment of lithium mica; Comparative Example 6 represents a high temperature roasting + sulfuric acid leaching treatment of spodumene + lithium mica; Compared with these six groups of comparative examples, the technical scheme of the present invention (Example 1) has the advantages of lower energy consumption, higher lithium extraction rate, simpler solution composition, and lower smelting slag amount, indicating that the technical scheme can lay a solid foundation for the efficient extraction of lithium from hard rock lithium ore, and has certain industrial promotion prospects.
[0079] The combination of high-temperature roasting and low-temperature sulfuric acid calcination of the present invention can cause interaction between spodumene and lepidolite ore. The high-temperature roasting and low-temperature sulfuric acid calcination cooperate with each other to fully expose the lithium in the spodumene and lepidolite ore and leach it through water. The main principle is that a very small amount of fluorine in the lepidolite attacks the spodumene mineral structure, so that the mineral is loosened and dissociated to a certain extent. However, if the sulfuric acid leaching process is directly adopted at this time (Comparative Example 6), the lithium extraction effect is also poor. The reason is that a very small amount of fluorine in the lepidolite attacks the spodumene mineral structure. Since no fluorine auxiliary agent is added, the lepidolite cannot completely dissociate the spodumene structure to expose lithium, so the lithium extraction is poor. However, if a very small amount of fluorine in the lepidolite attacks the spodumene mineral structure first, so that the mineral is loosened and dissociated to a certain extent, and then Combined with the sulfuric acid low-temperature calcination process, the spodumene structure that is loose and dissociated to a certain extent can be very quickly disintegrated from the ore to expose lithium during the subsequent acid low-temperature calcination, and continue to generate lithium sulfate with sulfuric acid, that is, the synergistic effect of fluorine attack and sulfuric acid low-temperature calcination, that is, acid calcination increases the attack effect of fluorine alone, and the fluorine attack effect increases the effect of acid calcination alone (Comparative Example 1 and Comparative Example 3 are compared with Example 1; Comparative Example 4, Comparative Example 5, Comparative Example 6 are compared with Example 1). The two process technologies cooperate with each other and have an excellent lithium extraction effect. In the case of high-temperature roasting of a single ore (without fluorine attack on lithium mica) + single acid calcination, and high-temperature roasting of a composite ore (with fluorine attack on lithium mica) + sulfuric acid leaching (without prior acid low-temperature calcination), the lithium extraction effect is poor.
[0080] In summary, the present invention discloses a method for efficiently extracting lithium by calcining spodumene lepidolite with sulfuric acid at low temperature, and the method comprises the following steps: first, uniformly mixing lepidolite concentrate with spodumene concentrate and then performing high-temperature roasting to obtain a roasting material; then, uniformly mixing the roasting material with sulfuric acid and performing low-temperature calcining to obtain an acidified material; finally, placing the acidified material in water for water leaching, and then performing solid-liquid separation to obtain a lithium leaching solution and lithium leaching tailings; the method utilizes the synergistic effect of high-temperature roasting (composite ore fluorine attack structure transformation) and low-temperature sulfuric acid calcination (disintegration of the transformed structure) to significantly improve the efficiency of lithium extraction from hard rock lithium ore; the lithium leaching rate is extremely high, while the leaching rates of impurity elements such as aluminum, sodium, potassium, etc. are low; the amount of smelting slag produced by the method for producing 1 ton of lithium carbonate product is reduced by about 50% compared with the traditional sulfate method; the technical solution has simple process, low energy consumption, low cost, is suitable for industrial application, and plays an extremely important role in the efficient development and utilization of lithium resources; and has excellent application and promotion prospects.
[0081] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.
Claims
1. A method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid, characterized in that: The lithium extraction method comprises the following steps: Step S1: uniformly mixing the lepidolite concentrate and the spodumene concentrate and then calcining them at high temperature to obtain a calcined material; Step S2: uniformly mixing the roasted material in step S1 with sulfuric acid, and calcining at low temperature to obtain an acidified material; Step S3: placing the acidified material in step S2 in water for water leaching, and then performing solid-liquid separation to obtain lithium leaching solution and lithium leaching tailings; The lithium mica concentrate is one or two of ferrolithium mica and lithium mica; The lithium content of the lepidolite concentrate is 0.3-2.0wt%; the lithium content of the spodumene concentrate is 1.5-3.7wt%; The mixing mass ratio of the lepidolite concentrate and the spodumene concentrate is 0.1:1 to 3.0:1; The high temperature roasting temperature in step S1 is 800-950°C; The high temperature roasting time in step S1 is 30 to 90 minutes; The temperature of low temperature calcination in step S2 is 150-300°C; The low temperature calcination time in step S2 is 10 to 60 minutes; The sulfuric acid is concentrated sulfuric acid.
2. A method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid as described in claim 1, characterized in that: The amount of the roasting material mixed with sulfuric acid in step S2 is 1.2 to 1.5 times the theoretical acid consumption when all the lithium elements in the spodumene lepidolite concentrate are converted into lithium sulfate.
3. A method for efficiently extracting lithium by low-temperature calcination of spodumene lepidolite with sulfuric acid as described in claim 1, characterized in that: The water immersion reaction conditions in step S3 are: liquid-to-solid ratio of 2-8 mL:1 g, temperature of 20-80° C., and time of 30-90 min.
Citation Information
Patent Citations
Method for lepidolite calcination treatment through vitriol and lithium carbonate preparation
CN106755967A
Method for extracting lithium from lepidolite by using composite salt roasting-water leaching process
CN116445736A
Method and system for preparing lithium carbonate by roasting lepidolite composite sulfate
CN117776231A
Process for extracting lithium from lithium pyroxene concentrate by using fluorine chemistry
CN102417995A
Method for acidizing spodumene to leach lithium
CN114436300A