A rapid evaluation method for atmospheric corrosion resistance of steel surface protective materials

By simulating different service environments in the periodic infiltrating environment test chamber, and combining accelerated corrosion test and protection coefficient correction, a rapid evaluation model was established, which solved the problem of difficult to quickly evaluate the corrosion resistance of steel materials and their surface protective materials in the prior art. The corrosion resistance evaluation and life expectancy prediction of the entire process of steel materials has been achieved, and the guidance of material development has been improved.

CN118641469BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD

Patent Information

Application Number
CN202411118915.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing technology is difficult to quickly and easily evaluate the corrosion resistance of steel materials and their surface iron oxide sheets, modified surfaces and protective coatings, and it is impossible to achieve corrosion resistance evaluation of the entire process of steel materials from substrate to protection system. This has led to the limitations on the application and development of steel materials.

Method used

The periodic infiltration environment test chamber is used to simulate different service environments, and the evaluation model is established through accelerated corrosion test, correlation analysis and protection coefficient correction, and the evaluation model is established to achieve a rapid evaluation of corrosion resistance such as iron oxide sheet, modified surface and protective coating on the surface of steel materials. and life expectancy.

Benefits of technology

It has achieved rapid evaluation and life prediction of corrosion resistance of steel materials and their protective surfaces, provided guidance on the research and development of steel materials and selection of protection systems, and filled the research gap in the field of surface oxidized iron sheets and modified surface corrosion evaluation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118641469B_ABST
    Figure CN118641469B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials. Different service environments and service conditions are simulated in a periodic infiltration environmental test box to rapidly evaluate corrosion resistance, and the evaluation results are corrected using a protection factor to establish an evaluation model to achieve rapid evaluation and life prediction of corrosion resistance of iron oxide scale, modified surface and protective coating on the material surface. Through the method of the present invention, the corrosion resistance of steel protective surfaces in different service environments and service conditions can be quantitatively evaluated, and the corrosion resistance evaluation and life prediction of the entire process of the same steel material from the steel substrate to the surface protection system can be achieved, providing guidance for the regulation of iron oxide scale on the surface of steel materials and the design of surface protection measures, while filling the research gap in the field of surface iron oxide scale and modified surface corrosion evaluation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material corrosion evaluation, and in particular relates to a method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials. Specifically, the present invention is a test method for conducting accelerated corrosion tests on materials such as steel substrates, surface iron oxide scale, modified surfaces and protective coatings in a laboratory using a circumferential immersion test chamber, and realizing rapid evaluation of material corrosion resistance by establishing a protection factor evaluation model. Background Art

[0002] The corrosion of steel materials in the environment has attracted much attention. Corrosion not only causes waste of resources and energy, but also causes corrosion failure of steel materials, which greatly endangers people's production and life. Among the various types of corrosion suffered by steel materials, atmospheric corrosion is the most serious and common, and the loss of steel materials caused by it accounts for more than 50% of the total corrosion loss. The temperature and humidity characteristics of the atmospheric environment make the surface of steel materials often in an environment of alternating day and night and dry and wet cycles. A layer of electrolyte liquid film will also condense on the surface of steel materials. With the participation of electrolytes in the liquid film, the corrosion of steel materials has electrochemical properties.

[0003] Effective assessment of corrosion life is one of the important factors limiting the application and development of steel materials. At present, the life assessment of steel materials mainly includes two aspects: actual environment coupon exposure test and laboratory accelerated corrosion test. The former has high accuracy, long test cycle and high cost, while the latter includes methods such as salt spray test and weekly immersion test. Among them, the salt spray test only strengthens a single environmental factor to achieve acceleration, and does not have functions such as dry-wet alternation. The simulation effect of the actual atmospheric environment and the correlation between indoor and outdoor are poor. The data change law of the weekly immersion test is closer to the real environment test data, and can simulate the characteristics of dry-wet alternation of atmospheric corrosion. It can reproduce the three atmospheric corrosion states of infiltration-humidity-dryness experienced by the metal surface, and has good simulation and acceleration.

[0004] At present, the rapid evaluation of corrosion resistance and life prediction of steel materials are mainly based on the steel material matrix. The evaluation results are only the corrosion resistance of the substrate, and it is impossible to evaluate the corrosion resistance of surface oxide scale, modified surface and protective coating with protective performance. In order to meet the application and development requirements of steel materials and their protection methods, there is an urgent need for a fast and simple method to quickly evaluate the corrosion resistance and life prediction of steel materials and their surface oxide scale, modified surface and protective coating and other surface protection materials, to achieve the corrosion resistance evaluation of the same steel material from the steel substrate to the surface protection system, and provide guidance for the research and development of steel materials and the selection and development of their protection systems. Summary of the invention

[0005] The present invention provides a method for rapidly evaluating the atmospheric corrosion resistance of steel surface protective materials. The method can rapidly evaluate the corrosion resistance of surface protective materials such as surface oxide scale, modified surface and protective coating of steel materials, realize the prediction of material corrosion life, and can be applied to the field of material corrosion resistance performance evaluation.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In order to solve the problem of rapid corrosion evaluation and life prediction of materials, the present invention provides a method for rapid atmospheric corrosion resistance evaluation of steel surface protective materials in view of the deficiencies in the prior art. More specifically, the method simulates different service environments and service conditions in a periodic infiltration environment test chamber to rapidly evaluate the corrosion resistance, and uses the protection factor to correct the evaluation results, establishes an evaluation model, and realizes rapid evaluation and life prediction of the corrosion resistance of the material surface oxide scale, modified surface and protective coating. The specific technical scheme is as follows:

[0008] A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials, the test process is: sample pretreatment, accelerated corrosion test, correlation analysis, protection factor correction, corrosion rapid evaluation, the specific method includes:

[0009] 1) Accelerated corrosion test: In the laboratory, the pre-treated samples are placed in a periodic immersion environment test chamber for multi-cycle accelerated corrosion test. After each cycle, the samples are characterized for microscopic morphology and product composition, and the corrosion rate and weight loss are calculated;

[0010] 2) Correlation analysis: For the steel material matrix, outdoor atmospheric exposure test was carried out according to GB / 14165-2008 "General requirements for field tests of atmospheric corrosion test of metals and alloys". After each cycle, the samples were characterized for microscopic morphology and product composition, and the corrosion rate and weight loss were calculated to obtain environmental spectrum data, and the correlation analysis was carried out with the laboratory accelerated corrosion test results: the power function model △W= At n Regression corrosion data, where: △W is the weight loss from corrosion, mm; t is the time, d; A is a constant; the corrosion kinetic curve of the accelerated corrosion test △W= At n And the corrosion kinetic curve of outdoor atmospheric exposure test △W0= A 0 t m , △W0 is the weight loss from corrosion in outdoor atmospheric exposure test, mm; A 0 is a constant; the grey correlation method is used to calculate and analyze the correlation between the two. If the grey correlation degree is greater than 0.6, it means that there is a good correlation between the two. That is, the corrosion kinetics curve of the accelerated corrosion test obtained is △W= Atn It is reasonable and can be used as a rapid evaluation model for steel material matrix in simulated service environment;

[0011] 3) Correction of protection factor: For surface protection materials with protective effects, accelerated tests are carried out under the same simulated environment as their steel substrates to obtain corrosion kinetic curves. The corrosion kinetic curves of the surface protection materials are compared with those of the steel substrates to calculate the protection factor γ. The rapid evaluation model is corrected with the protection factor to obtain the corrected rapid evaluation model △W= γAt n ,in γ <1 indicates that the surface treatment has a protective effect; γ≥1 indicates that the surface treatment has no protective effect;

[0012] 4) Rapid corrosion evaluation: Rapid evaluation models are used to conduct rapid corrosion evaluation of materials, including corrosion resistance prediction, corrosion life prediction and protective performance evaluation.

[0013] Surface protection materials with protective functions include iron oxide scale, modified surface and protective coating.

[0014] The periodic immersion environmental test chamber shall have temperature and humidity adjustment functions. The environmental conditions in the test chamber shall be set according to the actual service environment of the material to simulate the service conditions in different regions and seasons: 2-5wt% NaCl solution is recommended for simulating marine atmospheric environment; 0.005-0.02 mol / L NaHSO3 solution is recommended for simulating industrial atmospheric environment; (1-3wt%) NaCl+(0.005-0.02mol / L) NaHSO3 solution is recommended for simulating industrial marine atmospheric environment, and pH = 3-5 is adjusted with dilute hydrochloric acid; 0.1-1wt% NaCl solution is recommended for simulating urban atmospheric environment, or it can be set according to the actual meteorological environmental parameters of the service environment; the air temperature of the periodic immersion environmental test chamber is set to 35-75°C, the solution temperature is 35-75°C, the humidity is 30-90%RH, and the dry-wet ratio is 3:1-5:1; 3-10 test cycles are recommended, and the total test duration is 7-30 days.

[0015] In the correlation analysis step, it is necessary to conduct an outdoor atmospheric exposure test on the steel material matrix to obtain environmental spectrum data. The environment selects typical marine, industrial, industrial marine and inland atmospheric environments, or selects the actual service environment. The test is only performed on the steel material matrix, and the evaluation of the surface protection material corresponding to the same steel material matrix uses the environmental spectrum data of its matrix.

[0016] In the protection factor correction step, the initial, late and average corrosion weight loss of the steel material matrix and the surface protection material are calculated respectively, and the corrosion dynamics curves of the surface protection material and the steel material matrix are compared to obtain the initial protection factor respectively. γ f , Late protection factor γ b and the average protection factor γ a , the rapid assessment model is modified by the protection factor, and the modified rapid assessment model △W= γAt n , γ take γ f 、γ b or γ a .

[0017] The sample pretreatment includes: processing, degreasing, cleaning, grinding and other necessary treatments on the test samples, and weighing the pretreated samples; among them, the steel material matrix is ​​treated in accordance with the national standard; the steel material with iron oxide scale is edge-sealed after cutting; the surface modified and protective coating samples are directly subjected to surface modification and coating operations on the steel material matrix; the mass and length, width and height dimensions of the test samples are measured.

[0018] In the corrosion rapid evaluation step, a rapid evaluation model is selected or modified according to the type of material to be evaluated, and the corrosion life of the material in the actual service environment can be predicted through short-term laboratory tests to achieve rapid evaluation of the corrosion of hot-rolled steel plates. The evaluation is divided into three categories:

[0019] 1) Corrosion resistance prediction: predict the corrosion resistance of materials in service environment; the specific method is: adopt a rapid evaluation method with an acceleration ratio of n, predict the corrosion weight loss and corrosion rate parameters of the material after n×m days through m days of laboratory test time, and predict and evaluate the corrosion resistance of the material.

[0020] 2) Corrosion life prediction: Under the premise of specifying the corrosion allowance, predict the corrosion life of the material; the specific method is: the corrosion allowance of the material is required to be Bmm, and the test cycle when the corrosion thinning Bmm is measured in the laboratory by a rapid evaluation method, and then multiplied by the acceleration ratio to predict the actual service life.

[0021] 3) Evaluation of protective performance: Rapidly evaluate the same type of steel material substrate and its protective surface (surface oxide scale with protective function, modified surface and protective coating) at the same time, and use correction coefficient to evaluate the protective performance of various protective surfaces.

[0022] The acceleration ratio is: when the corrosion weight loss of the outdoor atmospheric exposure test is equal to that of the laboratory accelerated corrosion test, the ratio of the time used for the two tests.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] Through the rapid evaluation method of atmospheric corrosion resistance of steel surface protective materials of the present invention, the corrosion resistance of the protective surface in different service environments and service conditions can be quantitatively evaluated, and the corrosion resistance evaluation and life prediction of the same steel material from the steel substrate to the surface protection system can be realized, and guidance can be provided for the regulation of iron oxide scale on the surface of steel materials and the design of surface protection measures, while filling the research gap in the field of surface iron oxide scale and modified surface corrosion evaluation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a flow chart of the rapid evaluation method of atmospheric corrosion resistance of steel surface protective materials. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the specific implementation methods of the present invention are further described below in conjunction with embodiments. The following embodiments are used to specifically illustrate the contents of the present invention. These embodiments are only general descriptions of the contents of the present invention and do not limit the contents of the present invention.

[0027] A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials, the test process is: sample pretreatment, accelerated corrosion test, correlation analysis, protection factor correction, corrosion rapid evaluation, the specific method includes:

[0028] 1) Accelerated corrosion test: In the laboratory, the pre-treated samples are placed in a periodic immersion environment test chamber for multi-cycle accelerated corrosion test. After each cycle, the microscopic morphology and product composition of the samples are characterized, and the corrosion rate and weight loss are calculated.

[0029] The simulated service conditions of the periodic immersion environmental test chamber are as follows: 2-5wt% NaCl solution is used to simulate the marine atmospheric environment; 0.005-0.02 mol / L NaHSO3 solution is used to simulate the industrial atmospheric environment; (1-3)wt% NaCl+(0.005-0.02)mol / L NaHSO3 solution is used to simulate the industrial marine atmospheric environment, and the pH value is adjusted to 3-5 with dilute hydrochloric acid; 0.1-1wt% NaCl solution is used to simulate the urban atmospheric environment, or it can be set according to the actual meteorological environmental parameters of the service environment; the air temperature of the periodic immersion environmental test chamber is set to 35-75°C, the solution temperature is 35-75°C, the humidity is 30-90%RH, and the dry-wet ratio is 3:1-5:1; the test cycle is 3-10 cycles, and the total test time is 7-30 days.

[0030] 2) Correlation analysis: For the steel material matrix, outdoor atmospheric exposure test was carried out according to GB / 14165-2008 "General requirements for field tests of atmospheric corrosion test of metals and alloys". After each cycle, the samples were characterized for microscopic morphology and product composition, and the corrosion rate and weight loss were calculated to obtain environmental spectrum data, and the correlation analysis was carried out with the laboratory accelerated corrosion test results: the power function model △W= At n Regression corrosion data, where: △W is the weight loss from corrosion, mm; t is the time, d; A is a constant; the corrosion kinetic curve of the accelerated corrosion test △W= At n And the corrosion kinetic curve of outdoor atmospheric exposure test △W0= A 0 t m , △W0 is the weight loss from corrosion in outdoor atmospheric exposure test, mm; A 0 is a constant; the grey correlation method is used to calculate and analyze the correlation between the two. If the grey correlation degree is greater than 0.6, it means that there is a good correlation between the two, that is, the corrosion kinetics curve of the accelerated corrosion test obtained is △W= At n It is reasonable and can be used as a rapid evaluation model for steel material matrix in simulated service environment.

[0031] The outdoor atmospheric exposure test environment selects typical marine, industrial, industrial marine and inland atmospheric environments, or selects the actual service environment. The evaluation of the surface protection material corresponding to the same steel material matrix adopts the environmental spectrum data of its matrix.

[0032] 3) Correction of protection factor: For steel material matrix samples, no correction is required, and the rapid evaluation model in step 2) is directly used; for surface protection materials with protective effects (oxidized iron sheets, modified surfaces, protective coatings, etc.), accelerated tests are carried out under the same simulated environment as their steel material matrix to obtain corrosion kinetic curves, and the corrosion kinetic curves of the surface protection materials are compared with the corrosion kinetic curves of the steel material matrix to calculate the protection factor γ, and the rapid evaluation model is corrected with the protection factor to obtain the corrected rapid evaluation model △W= γAt n ,in γ <1 indicates that the surface treatment has a protective effect; γ≥1 indicates that the surface treatment has no protective effect.

[0033] More preferably, the initial, late and average corrosion weight loss of the steel material matrix and the surface protection material are calculated respectively, and the corrosion dynamics curves of the surface protection material and the steel material matrix are compared to obtain the initial protection coefficient γ f, Late protection factor γ b and the average protection factor γ a , the rapid assessment model is modified by the protection factor, and the modified rapid assessment model △W= γAt n , γ take γ f 、γ b or γ a ,like γ <1 indicates that the surface treatment has a protective effect; γ≥1 indicates that the surface treatment has no protective effect.

[0034] 4) Rapid corrosion evaluation: Rapid corrosion evaluation of materials is performed using a rapid evaluation model, including corrosion resistance prediction, corrosion life prediction, and protection performance evaluation. The specific evaluation is divided into the following three categories:

[0035] a) Corrosion resistance prediction: predict the corrosion resistance of materials in service environment; the specific method is: using a rapid evaluation method with an acceleration ratio of n, predict the corrosion weight loss and corrosion rate parameters of the material after n×m days through a laboratory test time of m days, and predict and evaluate the corrosion resistance of the material;

[0036] b) Corrosion life prediction: Under the premise of specifying the corrosion allowance, predict the corrosion life of the material; the specific method is: the corrosion allowance of the material is required to be Bmm, and the test cycle when the corrosion thinning Bmm is measured in the laboratory by a rapid evaluation method, and then multiplied by the acceleration ratio to predict the actual service life;

[0037] c) Evaluation of protective performance: Rapidly evaluate the same type of steel material substrate and its protective surface at the same time, and use correction factors to evaluate the protective performance of various protective surfaces.

[0038] The sample pretreatment method is: processing, degreasing, cleaning, and grinding the test samples, and weighing the pretreated samples; among them, the steel material matrix is ​​processed in accordance with the national standard; the steel material with iron oxide scale is edge-sealed after cutting; the surface modified and protective coating samples are directly subjected to surface modification and coating operations on the steel material matrix; the mass and length, width, and height dimensions of the test samples are measured.

[0039] Embodiment 1:

[0040] The method of the present invention is used to evaluate the surface iron oxide. DH32 with two kinds of iron oxide produced by different processes is evaluated. Iron oxide I is dense and iron oxide II is loose. The sample is cut into 50mm*50mm*5mm test pieces without damaging the surface iron sheet, and the edge is sealed after cutting. A 3.5wt% NaCl solution simulating the marine atmospheric environment is used. The test environment temperature is 35°C, the solution temperature is 45°C, and the humidity is 70±5%RH. Each dry-wet cycle is 60 min, the dry-wet ratio is 5:1, the test cycle is 10 cycles, and the total test duration is 15 days. At the same time, indoor accelerated tests are carried out on DH32 matrix samples, iron oxide I samples, and iron oxide II samples. The corrosion kinetics data are fitted with a power function, and the laboratory accelerated test data are correlated with the atmospheric exposure test data of DH32 steel at the Hainan Corrosion Test Station. The microscopic morphology and product composition of the samples in each cycle indoor and outdoor are similar; the gray correlation degree of the accelerated test and outdoor exposure test of the DH32 steel matrix in the simulated solution is calculated to be 0.8, and the corrosion dynamics of the two are consistent. The calculated acceleration ratio is 29, the protection factor γ of the oxide scale I is 0.79, and the protection factor γ of the oxide scale II is 0.88, both of which are less than 1, indicating that the oxide scale has a protective effect on the DH32 matrix steel, and the dense oxide scale I with a smaller protection factor has better protection performance.

[0041] Embodiment 2:

[0042] The modified surface is evaluated by the method of the present invention. The super-hydrophobic modified surface of ship plate steel A plate is evaluated, the ship plate steel A sample is cut into 50mm*50mm*5mm test pieces, and the surface is super-hydrophobic modified to obtain etched surface I and deposited surface II. A 0.01 mol / L NaHSO3 solution simulating an industrial atmospheric environment is used, the test environment temperature is 75°C, the solution temperature is 75°C, the humidity is 90±5%RH, each dry-wet cycle is 60min, the dry-wet ratio is 3:1, the test cycle is 5 cycles, and the total test duration is 30 days. At the same time, laboratory accelerated tests are carried out on the ship plate steel A matrix sample and the super-hydrophobic surface modified sample samples I and II. The corrosion kinetics data are fitted with a power function, and the laboratory accelerated test data are correlated with the atmospheric exposure test data of ship plate steel A at the Chongqing Corrosion Test Station. The microscopic morphology and product composition of the samples in each cycle indoor and outdoor are similar; the gray correlation degree of the accelerated test and outdoor exposure test of the ship plate steel A matrix in the simulated solution is calculated to be 0.78, and the corrosion dynamics of the two are consistent. The calculated acceleration ratio is 41, the protection factor γ of the etched surface I is 0.48, and the protection factor γ of the deposited surface II is 0.56. The protection factor γ is less than 1, indicating that the superhydrophobic modified surface substrate steel has a protective effect, and the etched surface I with a smaller protection factor has better protection performance. Under the premise of a specified corrosion allowance of 5 mm, the two modified surfaces can increase the corrosion life by 2.08 times and 1.79 times, respectively.

[0043] Embodiment 3:

[0044] The method of the present invention is used to evaluate the protective coating. The corrosion resistance of the epoxy coating on the surface of Q345 steel is evaluated. The Q345 steel sample is cut into 50mm*50mm*5mm test pieces, and the surface is coated with epoxy coating. A 2wt% NaCl+0.01mol / L NaHSO3 solution simulating the industrial marine atmospheric environment is used, and the pH = 4 is adjusted with dilute hydrochloric acid. The test environment temperature is 45°C, the solution temperature is 45°C, and the humidity is 70±5%RH. Each dry-wet cycle is 60 min, the dry-wet ratio is 4:1, the test cycle is 5 cycles, and the total test duration is 15 days. At the same time, laboratory accelerated tests are performed on Q345 steel substrate samples and coated coating sample samples. The corrosion kinetics data are fitted with a power function, and the laboratory accelerated test data are correlated with the atmospheric exposure test data of Q345 steel at the Qingdao Corrosion Test Station. The microscopic morphology and product composition of the samples in each cycle indoor and outdoor are similar; the gray correlation between the accelerated test and the outdoor exposure test of the Q345 steel substrate in the simulated solution is calculated to be 0.85, and the corrosion dynamics of the two are consistent. The calculated acceleration ratio is 33, the protection factor γ of the epoxy coating is 0.38, and the protection factor γ is less than 1, indicating that the surface coating has a protective effect. After correction of the acceleration ratio and protection factor, the corrosion weight loss and corrosion rate of the steel substrate and epoxy coating exposed outdoors for half a year can be predicted in the laboratory for 132h and 349h respectively.

Claims

1. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials, characterized in that: The test process is: sample pretreatment, accelerated corrosion test, correlation analysis, protection factor correction, and corrosion rapid evaluation. The specific methods include: 1) Accelerated corrosion test: In the laboratory, the pre-treated samples are placed in a periodic immersion environment test chamber for multi-cycle accelerated corrosion test. After each cycle, the samples are characterized for microscopic morphology and product composition, and the corrosion rate and weight loss are calculated; 2) Correlation analysis: For the steel material matrix, outdoor atmospheric exposure test was carried out according to GB / 14165-2008 "General requirements for field tests of atmospheric corrosion test of metals and alloys". After each cycle, the samples were characterized for microscopic morphology and product composition, and the corrosion rate and weight loss were calculated to obtain environmental spectrum data, and the correlation analysis was carried out with the laboratory accelerated corrosion test results: the power function model △W= At n Regression corrosion data, where: △W is the weight loss from corrosion, mm; t is the time, d; A is a constant; the corrosion kinetic curve of the accelerated corrosion test △W= At n And the corrosion kinetic curve of outdoor atmospheric exposure test △W0= A 0 t m , △W0 is the weight loss from corrosion in outdoor atmospheric exposure test, mm; A 0 is a constant; the grey correlation method is used to calculate and analyze the correlation between the two. If the grey correlation degree is greater than 0.6, it means that there is a good correlation between the two, that is, the corrosion kinetics curve of the accelerated corrosion test obtained is △W= At n It is reasonable and can be used as a rapid evaluation model for steel material matrix in simulated service environment; 3) Correction of protection factor: For surface protection materials with protective effects, accelerated tests are carried out under the same simulated environment as their steel substrates to obtain corrosion kinetic curves. The corrosion kinetic curves of the surface protection materials are compared with those of the steel substrates to calculate the protection factor γ. The rapid evaluation model is corrected with the protection factor to obtain the corrected rapid evaluation model △W= γAt n ,in γ <1 indicates that the surface treatment has a protective effect; γ≥1 indicates that the surface treatment has no protective effect; 4) Rapid corrosion evaluation: Rapid evaluation models are used to conduct rapid corrosion evaluation of materials, including corrosion resistance prediction, corrosion life prediction and protective performance evaluation.

2. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 1, characterized in that: Surface protection materials with protective functions include iron oxide scale, modified surface and protective coating.

3. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 1, characterized in that: The simulated service conditions of the cyclic immersion environmental test chamber are as follows: 2-5wt% NaCl solution is used to simulate the marine atmospheric environment; 0.005-0.02 mol / L NaHSO3 solution is used to simulate the industrial atmospheric environment; (1-3)wt% NaCl+(0.005-0.02)mol / L NaHSO3 solution is used to simulate the industrial marine atmospheric environment, and the pH value is adjusted to 3-5 with dilute hydrochloric acid; 0.1-1wt% NaCl solution is used to simulate the urban atmospheric environment, or it can be set according to the actual meteorological environmental parameters of the service environment; the air temperature of the cyclic immersion environmental test chamber is set to 35-75°C, the solution temperature is 35-75°C, the humidity is 30-90%RH, and the dry-wet ratio is 3:1-5:1; the test cycle is 3-10 cycles, and the total test time is 7-30 days.

4. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 1, characterized in that: In the correlation analysis step, the outdoor atmospheric exposure test environment selects typical marine, industrial, industrial marine and inland atmospheric environments, or selects an actual service environment.

5. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 1, characterized in that: In the protection factor correction step, the initial, late and average corrosion weight loss of the steel material matrix and the surface protection material are calculated respectively, and the corrosion dynamics curves of the surface protection material and the steel material matrix are compared to obtain the initial protection factor respectively. γ f , Late protection factor γ b and the average protection factor γ a , the rapid assessment model is modified by the protection factor, and the modified rapid assessment model △W= γAt n , γ Take γ f , γ b or γ a .

6. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 1, characterized in that: The sample pretreatment includes: processing, degreasing, cleaning, and grinding the test samples, and weighing the pretreated samples; the steel material matrix is ​​processed according to the national standard; the steel material with iron oxide is edge-sealed after cutting; the surface modified and protective coating samples are directly subjected to surface modification and coating operations on the steel material matrix; and the mass and length, width, and height dimensions of the test samples are measured.

7. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 1, characterized in that: In the corrosion rapid evaluation step, the evaluation is divided into three categories: 1) Corrosion resistance prediction: predict the corrosion resistance of materials in service environment; the specific method is: adopt a rapid evaluation method with an acceleration ratio of n, predict the corrosion weight loss and corrosion rate parameters of materials after n×m days through a laboratory test time of m days, and predict and evaluate the corrosion resistance of materials; 2) Corrosion life prediction: Under the premise of specifying the corrosion allowance, predict the corrosion life of the material; the specific method is: the corrosion allowance of the material is required to be Bmm, and the test cycle when the corrosion thinning Bmm is measured in the laboratory by a rapid evaluation method, and then multiplied by the acceleration ratio to predict the actual service life; 3) Evaluation of protective performance: Rapidly evaluate the same type of steel material substrate and its protective surface at the same time, and use correction factors to evaluate the protective performance of various protective surfaces.

8. A method for rapid evaluation of atmospheric corrosion resistance of steel surface protective materials according to claim 7, characterized in that: The acceleration ratio is: when the corrosion weight loss of the outdoor atmospheric exposure test is equal to that of the laboratory accelerated corrosion test, the ratio of the time used for the two tests.

Citation Information

Patent Citations

  • Marine atmosphere simulated accelerated testing method for coating

    CN103954550A

  • Indoor and outdoor corrosion test correlation analysis method

    CN114383997A

  • Corrosion test condition calculation method and device

    CN115855791A

Cited By

  • Detection system and comprehensive evaluation method for marine transportation anti-corrosion duration of protective material

    CN120971308A

  • A detection system and comprehensive evaluation method for marine corrosion prevention duration of protective material

    CN120971308B

  • Marine atmospheric environment corrosion evaluation system and method

    CN121090392A