Waterproof and breathable fabric and preparation method thereof
By using a three-layer block copolymer film layer and hydrophilic flexible gauze in the waterproof fabric, combined with a nylon waterproof layer, the problem of waterproof and moisture permeability is difficult to take into account, and waterproof and moisture permeability in high temperature and high humidity environments are achieved Performance improvements and comfort improvements.
Patent Information
- Application Number
- CN202411132912.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing waterproof fabrics have poor moisture permeability in high temperature and high humidity environments, resulting in a stuffy and hot feeling, and it is difficult to take into account both waterproof and moisture permeability.
The block copolymer film layer with a three-layer structure and a hydrophilic flexible gauze are used, combined with a nylon waterproof layer, and the waterproof and moisture-permeable properties of the fabric are optimized through the multi-layer structure and swelling treatment of the block copolymer film layer.
In high temperature and high humidity environments, the waterproof performance and moisture permeability are improved, which relieves the sultry feeling and enhances the comfort of the fabric.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of fabrics, and in particular relates to a waterproof and breathable fabric. Background Art
[0002] At present, waterproof fabrics usually reduce the air permeability of fabrics, increase hydrophobicity, etc., thereby improving waterproof performance. Breathable fabrics increase the air permeability and moisture absorption of fabrics. In fact, waterproof and breathable are almost opposite properties in actual use. Usually waterproof fabrics tend to have poor breathability, and breathable fabrics have poor waterproof performance. In the face of summer, especially in the high temperature and high humidity environment in the south in summer, waterproof fabrics have a strong sense of stuffiness after wearing.
[0003] For example, patent application CN117757407A improves the two properties of sun protection and waterproofing in order to obtain a fabric that meets the requirements of rain and sun protection. The laminating layer used is waterproof and has a moisture permeability function. However, the moisture permeability of the fabric cannot be adaptively adjusted on hot and rainy days, or is reduced to a certain extent.
[0004] For example, patent application CN117621584A relates to a modified polytetrafluoroethylene microporous membrane with waterproof and breathable functions. In fact, in high humidity weather such as rain, the performance of this fabric is poor and it is more suitable for sunny days. Summary of the invention
[0005] In order to solve the above problems, the present application provides a waterproof and breathable fabric and a preparation method thereof.
[0006] The fabric has excellent waterproof and breathable properties. In rainy / hot and muggy environments, it has adaptive breathable properties, which can alleviate the stuffiness caused by wearing the fabric in hot and muggy rainy environments.
[0007] In a first aspect, the present invention provides a method for preparing a waterproof and breathable fabric, wherein the outer layer of the waterproof and breathable fabric is a nylon waterproof layer, the inner layer is a hydrophilic flexible gauze, the middle layer is a block copolymer film layer, and the block copolymer film layer is a PEG / PSF- b -PEG blended membrane layer, in the order from the outer layer to the inner layer of the waterproof and breathable fabric, the outermost layer of the block copolymer membrane layer is the first membrane layer structure, the middle layer is the second membrane layer structure, and the innermost layer is the third membrane layer structure; the preparation method comprises the following steps:
[0008] Step 1: prepare a block copolymer film solution, dissolve the constituent materials of the first film structure in a benign solvent to obtain a first solution, dissolve the constituent materials of the second film structure in a benign solvent to obtain a second solution, and dissolve the constituent materials of the third film structure in a benign solvent to obtain a third solution, wherein the constituent material of the first film structure is PSF-b -PEG block copolymer, the constituent material of the second membrane structure is PEG homopolymer or PSF in which the mass ratio of PEG homopolymer and PSF is 70%-85%. b -PEG block copolymer mixture, wherein the mass proportion of PEG homopolymer in the mixture is 80%-90%, and the constituent material of the third membrane structure is PSF- wherein the mass proportion of PEG chain segment is 45%-60%. b -PEG block copolymers;
[0009] Step 2: Apply a certain amount of the first solution to the inner side of the nylon waterproof layer, and obtain a first film structure with a thickness of 5-10 μm on the inner side of the waterproof layer after the solvent evaporates naturally;
[0010] A certain amount of the second solution is applied to the inner side of the first film structure layer, and after the solvent evaporates naturally, a second film layer structure with a thickness of 15-20 μm is obtained on the inner side of the first film layer;
[0011] A certain amount of the third solution is applied to the inner side of the second film layer structure, and a hydrophilic flexible gauze is applied to the third solution. After the solvent evaporates, a third film layer structure with a thickness of 15-20 μm is obtained on the inner side of the first film layer. At the same time, a hydrophilic flexible gauze is attached to the inner side of the third film layer structure to obtain a water-proof moisture-permeable fabric;
[0012] Step 3: Place the above-mentioned waterproof and breathable fabric in an ethanol solution for swelling, the swelling temperature is 45-75°C, the swelling time is 5min-60min, and then take it out and dry it to obtain a waterproof and breathable fabric.
[0013] Furthermore, step 1 specifically includes a first solution with a mass fraction of 7wt%-10wt%, a second solution with a mass fraction of 15wt%-20wt%, and a third solution with a mass fraction of 10wt%-15wt%.
[0014] Furthermore, the benign solvent is chloroform.
[0015] Furthermore, the PSF- b -PEG block copolymer molecular weight is 75kDa-150kDa;
[0016] The third film structure consists of PSF- b -PEG block copolymer molecular weight is 100kDa-200kDa;
[0017] When the constituent material of the second membrane structure is a PEG homopolymer, the molecular weight of the homopolymer is 4000-7000Da; when the constituent material of the second membrane structure is a PEG homopolymer and a PSF- b-PEG block copolymer mixture, PEG homopolymer molecular weight is 5000-10000Da, PSF- b -PEG block copolymers have a molecular weight of 50 kDa-75 kDa.
[0018] In a second aspect, the present invention provides a waterproof and breathable fabric, which is prepared by the above method.
[0019] The beneficial effects of this application are as follows:
[0020] First, the waterproof and breathable fabric in this application is a composite material, the outer layer is a waterproof layer, which provides basic waterproof effect; the inner layer is a hydrophilic layer, which has a certain hygroscopicity and more importantly can ensure that the inner layer is comfortable and soft.
[0021] Second, the middle layer of the present application adopts a block copolymer film layer with a three-layer structure, wherein the first film layer structure can provide a certain waterproof performance, and with the wetting of rain or water vapor in the air, the PEG segment undergoes limited swelling, resulting in a reduction in the membrane pore gap; at the same time, since the proportion of the main chain segment PSF segment in the first film layer structure is much higher than that of the PEG segment, under the action of water molecules, the PEG segment's segment swelling and migration tendency at a microscopic level are limited by the PSF segment and cannot break through the constraints of the PSF segment, resulting in a reduction in the pore gap after the fabric is wetted, thereby further increasing the waterproof performance.
[0022] When the film-forming material of the second film layer is PEG homopolymer, it can provide a large number of water molecule channels and have a certain water storage function, thereby improving the moisture permeability. b -PEG block copolymers can further increase the moisture permeability after swelling. And PSF- b The introduction of -PEG chain segments can enhance the structural strength of the second membrane layer. Due to the subsequent swelling process, the PSF- b The -PEG chain segment can simultaneously increase the binding force between the second film layer and the first film layer, and between the second film layer and the third film layer.
[0023] The third film structure PSF- b -After the PEG is opened, it can diffuse water molecules to the second and first layers through microscopic pores; at the same time, when the temperature of the wearer's surrounding environment rises to 40°C or above, the water vapor emitted by the human body can produce a certain degree of swelling and segregation effect on the PEG chain segments. Under this effect, the volume of the PEG chain segments expands. Although the porosity will decrease, more PEG chain segments can migrate at the microscopic level and thus contact more water molecules, so more water molecules can be transmitted or retained. The moisture permeability is increased, which to a certain extent compensates for the decrease in moisture permeability caused by the improvement of the waterproof performance of the first layer.
[0024] Through the coordination of the three-layer structure, enhanced waterproof performance and improved moisture permeability can be obtained in high temperature and high humidity environments. After being made into clothing, the improvement of the waterproof performance and moisture permeability can bring significant improvement in wearing comfort to the wearer. DETAILED DESCRIPTION
[0025] Embodiment 1:
[0026] 1. Select PSF with a molecular weight of 75 kDa. b -PEG block copolymer, wherein the mass ratio of PSF to PEG segments is 85:15, is dissolved in chloroform to obtain a first solution with a mass fraction of 10%, and the solution is applied to the inner side of the nylon waterproof layer, and the chloroform is waited for volatilization to obtain a first membrane structure with a thickness of 5 μm;
[0027] 2. Select a PEG polymer with a molecular weight of 4000, dissolve it in chloroform to obtain a second solution with a concentration of 15 wt%, apply the solution to the inner side of the first film layer structure, and wait for the chloroform to evaporate to obtain a second film layer structure with a thickness of 15 μm;
[0028] 3. Select PSF with a molecular weight of 100 kDa b -PEG block copolymer, wherein the mass ratio of PSF:PEG chain segments is 55:45, dissolved in chloroform to obtain a third solution with a mass fraction of 10wt%, the solution is coated on the inner side of the second membrane layer structure, and hydrophilic flexible gauze is attached to the third solution, and after the solvent evaporates, a third membrane layer structure with a thickness of 15μm and hydrophilic flexible gauze attached to the inner side thereof are obtained to obtain a water-permeable fabric.
[0029] The fabric was placed in an ethanol solution for swelling at a temperature of 45°C for 45 minutes, and then taken out and air-dried to obtain a waterproof and breathable fabric.
[0030] Embodiment 2:
[0031] Compared with Example 1, the difference is that the swelling temperature is 45°C and the swelling time is 60min.
[0032] Comparative Example 1:
[0033] Compared with Example 1, the difference is that the swelling temperature is 45°C and the swelling time is 2h.
[0034] Embodiment 3:
[0035] Compared with Example 1, the difference is that the swelling temperature is 75°C and the swelling time is 5 min.
[0036] Embodiment 4:
[0037] Compared with Example 1, the difference is that the molecular weight in the first solution is PSF- b The molecular weight of the -PEG block copolymer is 150 kDa.
[0038] Comparative Example 2:
[0039] Compared with Example 1, the difference is that the first solution uses a PSF homopolymer with a molecular weight of 75 kDa.
[0040] Embodiment 5:
[0041] Compared with Example 1, the difference is that in the block copolymer in the first solution, the mass ratio of PSF:PEG segments is 95:5.
[0042] Comparative Example 3:
[0043] Compared with Example 1, the difference is that in the block copolymer in the first solution, the mass ratio of PSF:PEG segments is 80:20.
[0044] Embodiment 6:
[0045] Compared with Example 1, the difference is that the thickness of the first film layer structure is 10 μm.
[0046] Comparative Example 4:
[0047] Compared with Example 1, the difference is that the first film layer structure is 2 μm.
[0048] Comparative Example 5:
[0049] Compared with Example 1, the difference is that the first film layer structure is 20 μm.
[0050] Embodiment 7:
[0051] Compared with Example 1, the difference is that the molecular weight of PEG in the second solution is 7000 Da.
[0052] Comparative Example 6:
[0053] Compared with Example 1, the difference is that the molecular weight of PEG in the second solution is 9000 Da.
[0054] Comparative Example 7:
[0055] The difference compared with Example 1 is that the molecular weight of PEG in the second solution is 2000 Da.
[0056] Embodiment 8:
[0057] Compared with Example 1, the difference is that: PEG with a molecular weight of 5000Da and PSF- with a molecular weight of 50kDa and a mass ratio of PSF to PEG segments of 7:3 are selected. b-PEG block copolymer, according to PEG and PSF- b The second solution was prepared with a mass ratio of 8:2 for PEG.
[0058] Embodiment 9:
[0059] Compared with Example 8, the difference is that the molecular weight of PEG is 10000 Da.
[0060] Comparative Example 8:
[0061] Compared with Example 8, the difference is that the molecular weight of PEG is 4000 Da.
[0062] Comparative Example 9:
[0063] Compared with Example 8, the difference is that the mass ratio of the PSF and PEG segments is 5:5.
[0064] Embodiment 10:
[0065] Compared with Example 8, the difference is that PEG and PSF- b The mass ratio of PEG is 9:1.
[0066] Comparative Example 10:
[0067] Compared with Example 8, the difference is that PEG and PSF- b The mass ratio of -PEG is 9.5:0.5.
[0068] Comparative Example 11:
[0069] Compared with Example 8, the difference is that PEG and PSF- b The mass ratio of PEG is 7:3.
[0070] Embodiment 11:
[0071] Compared with Example 1, the difference is that PSF- b -PEG has a molecular weight of 200 kDa.
[0072] Comparative Example 12:
[0073] Compared with Example 1, the difference is that PSF- b -PEG has a molecular weight of 75 kDa.
[0074] Embodiment 12:
[0075] Compared with Example 1, the difference is that PSF- b The chain segment mass ratio of -PEG is PSF:PEG=40:60.
[0076] Comparative Example 13:
[0077] Compared with Example 1, the difference is that PSF- b The mass ratio of -PEG chain segments is PSF:PEG=30:70.
[0078] Comparative Example 14:
[0079] Compared with Example 1, the difference is that PSF- b The chain segment mass ratio of -PEG is PSF:PEG=65:35.
[0080] The moisture permeability test was carried out in accordance with GB / T12704.2-2009 standard, with reference to the experimental conditions of group b (temperature of (23±2)°C, relative humidity of (50±2)%, positive cup method experiment) as experimental condition 1;
[0081] In addition, in order to simulate a high temperature and high humidity environment, the second experimental condition was set. Compared with experimental condition 1, the difference was: the temperature was (40±2)°C, the relative humidity was (80±2)%. The unit of water vapor permeability was g / (m 2 ·24h), the waterproof performance refers to GB / T4745-2012. In addition, the fabric (unwashed fabric) is placed in an environment with a temperature of (40±2)°C and a relative humidity of (80±2)% for 12h, and then the waterproof performance is tested again in accordance with GB / T4745-2012 as the waterproof performance after wetting (the so-called wetting does not mean that the fabric is completely wet, in fact, the fabric cannot be seen to be wet by the naked eye after it is taken out).
[0082] For washing, refer to the 4N machine wash method in GB / T8629-2017, hang to dry, and wash three times.
[0083] The experimental results are as follows:
[0084]
[0085] From the analysis of Examples 1-3 and Comparative Example 1, it can be seen that too much swelling will lead to reduced waterproof performance and poor moisture permeability. The reason may be that after excessive swelling, the pores in the third layer of the membrane structure collapse during the use of the fabric, and at the same time, a strong microscopic phase transfer between PSF and PEG in the third layer of the membrane structure leads to the formation of a partial PSF macroscopic continuous phase inside the membrane layer, blocking part of the PEG water channel.
[0086] Through the analysis of Example 4 and Comparative Example 2, it can be seen that the increase in molecular weight improves the stability after machine washing. When PSF homopolymer is used, on the one hand, swelling segregation cannot be achieved, which makes the moisture permeability of the fabric poor and the actual waterproof performance is not improved. On the other hand, the increase in waterproof performance cannot be achieved when the humidity increases. In addition, when the molecular weight of the block copolymer used is too high, it will cause difficulty in opening the hole, and when the molecular weight is too low, it will cause poor stability after washing.
[0087] From the analysis of Example 5 and Comparative Example 3, it can be seen that as the mass proportion of the PSF chain segment in the first layer increases, the waterproof performance is significantly improved. However, when the PSF proportion is too low, such as reduced to 80%, the waterproof performance of the fabric will no longer change after being soaked in rainwater, but will remain unchanged. The reason may be that after the PSF chain segment is reduced, the PEG chain segment with a higher content may partially break through the PSF micro-continuous phase and contact the external water to absorb moisture.
[0088] From the analysis of Example 6 and Comparative Examples 4-5, it can be seen that the thickness of the first film layer directly affects the integrity of the block copolymer layer and the waterproof performance of the fabric. In fact, within a certain range, the increase in thickness can improve the waterproof performance of the fabric, but the change in film thickness has little effect on the moisture permeability. When the thickness is too low, the integrity of the fabric will be significantly reduced after multiple washings.
[0089] Moreover, if the film thickness increases excessively, such as to 20 μm, the waterproofness will no longer be significantly improved, but the moisture permeability will be significantly reduced.
[0090] Analysis of Example 7 and Comparative Examples 6-7 shows that the reduction of PEG molecular weight directly affects the stability after multiple washings. The reason may be that the low molecular weight leads to defects in the second layer, resulting in a decrease in waterproof performance. In addition, the high molecular weight causes a decrease in moisture permeability. The reason may be that the defects in the second film layer formed by high molecular weight PEG increase, and due to excessive entanglement between molecular weights, the resistance of water molecule channels increases, and the moisture permeability decreases slightly.
[0091] Analysis of Example 8 shows that the second film layer increases PSF- b -PEG block copolymer, the stability after washing is significantly increased. At the same time, the waterproof performance and moisture permeability are improved. The reason may be that after swelling, the second membrane layer produces microscopic pores, which increases the diffusion rate of water molecules and the space for accommodating water molecules. In addition, after swelling, the PSF chain segment segregates and moves to the first layer, blocking between the first and second layers, resulting in improved waterproof performance.
[0092] However, since the PEG chain segment is still a continuous phase at the microscopic level after swelling, the introduction of PSF does not weaken the water molecule transfer performance.
[0093] From the analysis of Example 9 and Comparative Example 8, it can be seen that the introduction of the PSF segment expands the molecular weight range of PEG applicable to the second layer, allowing the application of PEG with a larger molecular weight. PEG with a large molecular weight can improve stability without affecting waterproofness and moisture permeability. However, when PEG with a smaller molecular weight is used, the PSF is not fully wrapped after the PEG molecular weight is reduced, which easily leads to a decrease in waterproof performance.
[0094] Analysis of Comparative Example 9 shows that when the mass ratio of the PSF chain segments is reduced, the waterproof barrier effect is not improved compared with the case where only PEG is used to form the second film layer. The reason may be that when the PSF content is too low, it is difficult to form an effective waterproof barrier PSF continuous phase.
[0095] From the analysis of Example 10 and Comparative Examples 10-11, it can be seen that in the second film layer, the increase in the PEG mass ratio will increase the moisture permeability without significantly reducing the waterproof performance. When the PEG content is too high, the waterproof performance will be reduced, and the waterproof performance is almost the same as that of the second film layer composed of only PEG. However, although the PEG content is too low, the waterproof performance will increase, but the flux will be significantly reduced.
[0096] Analysis of Example 11 and Comparative Example 12 shows that as PSF- b -As the molecular weight of PEG increases, its waterproof performance improves slightly. When the molecular weight is too low (reduced to 75kDa), the entanglement between the molecular chains decreases. Although the hygroscopicity increases significantly, the water channels in the inner layer are too large, which affects the overall waterproof performance of the fabric and the waterproof grade decreases slightly.
[0097] From the analysis of Example 12 and Comparative Examples 13-14, it can be seen that as the proportion of PEG increases, the moisture permeability is improved to a certain extent. However, when the proportion of PSF in the third layer of the membrane structure is reduced to 30%, swelling will cause poor adhesion of the membrane layer, and the lack of PSF support will cause performance degradation after repeated use. However, when the proportion of PSF is too high (such as up to 65%), PSF forms a macroscopically local continuous phase after swelling, which makes the fabric lose the function of improving moisture permeability in high temperature and high humidity environments.
[0098] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing a waterproof and breathable fabric, wherein the outer layer of the waterproof and breathable fabric is a nylon waterproof layer, the inner layer is a hydrophilic flexible gauze, the middle layer is a block copolymer film layer, and the block copolymer film layer is a PEG / PSF- b -PEG blended membrane layer, in the order from outer layer to inner layer of the waterproof and breathable fabric, the outermost layer of the block copolymer membrane layer is the first membrane layer structure, the middle layer is the second membrane layer structure, and the innermost layer is the third membrane layer structure; characterized by: Step 1: prepare a block copolymer film solution, dissolve the constituent materials of the first film structure in a benign solvent to obtain a first solution, dissolve the constituent materials of the second film structure in a benign solvent to obtain a second solution, and dissolve the constituent materials of the third film structure in a benign solvent to obtain a third solution, wherein the constituent material of the first film structure is PSF- b -PEG block copolymer, the constituent material of the second membrane structure is PEG homopolymer or PSF in which the mass ratio of PEG homopolymer and PSF is 70%-85%. b -PEG block copolymer mixture, wherein the PEG homopolymer accounts for 80%-90% by weight, and the constituent material of the third membrane structure is PSF- wherein the PEG segment accounts for 45%-60% by weight. b -PEG block copolymer; PSF- b -PEG block copolymer has a molecular weight of 75kDa-150kDa; the constituent materials of the third membrane structure include PSF- b -PEG block copolymer molecular weight is 100kDa-200kDa; when the constituent material of the second membrane structure is PEG homopolymer, the molecular weight of the homopolymer is 4000-7000Da; the constituent material of the second membrane structure is PEG homopolymer and PSF with a mass ratio of 70%-85% of PSF- b -PEG block copolymer mixture, PEG homopolymer molecular weight is 5000-10000Da, PSF- b -PEG block copolymer molecular weight is 50kDa-75kDa; Step 2: Apply a certain amount of the first solution to the inner side of the nylon waterproof layer, and obtain a first film structure with a thickness of 5-10 μm on the inner side of the waterproof layer after the solvent evaporates naturally; A certain amount of the second solution is applied to the inner side of the first film structure layer, and after the solvent evaporates naturally, a second film layer structure with a thickness of 15-20 μm is obtained on the inner side of the first film layer; A certain amount of the third solution is applied to the inner side of the second film layer structure, and a hydrophilic flexible gauze is applied to the third solution. After the solvent evaporates, a third film layer structure with a thickness of 15-20 μm is obtained on the inner side of the first film layer. At the same time, a hydrophilic flexible gauze is attached to the inner side of the third film layer structure to obtain a water-proof moisture-permeable fabric; Step 3: Place the above-mentioned waterproof and breathable fabric in an ethanol solution for swelling, the swelling temperature is 45-75°C, the swelling time is 5min-60min, and then take it out and dry it to obtain a waterproof and breathable fabric.
2. The preparation method according to claim 1, wherein step 1 specifically comprises the mass fraction of the first solution being 7wt%-10wt%, the mass fraction of the second solution being 15wt%-20wt%, and the mass fraction of the third solution being 10wt%-15wt%.
3. The preparation method according to claim 2, wherein the benign solvent is chloroform.
4. A waterproof and breathable fabric, prepared by the method according to any one of claims 1 to 3.