A method and device for treating organic wastewater with microwave photocatalysis

By using a composite catalyst of modified cellulose-based activated carbon fiber and Fe2O3 nanoparticles, combined with micro-nano bubbles and microwave radiation technology, the problem of narrow ultraviolet absorption range of photocatalysts is solved, significantly improving the degradation ability of organic wastewater, and satisfying the large Process requirements at scale.

CN118651929BActive Publication Date: 2024-11-26SHAANXI SCI TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411131573.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The ultraviolet light absorption range of existing photocatalysts is relatively narrow, and their ability to degrade organic pollutants is weak, making it difficult to meet the treatment needs of large-scale industrial wastewater.

Method used

Compound catalysts, including cellulose-based activated carbon fibers and Fe2O3 nanoparticles, are used to improve photocatalytic performance through modification treatment, and combine micro-nano bubbles and microwave radiation technology to form a blended system for processing.

Benefits of technology

The light absorption range and active sites of the photocatalyst are significantly improved, the degradation capacity of organic pollutants is enhanced, and efficient organic wastewater treatment is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118651929B_ABST
    Figure CN118651929B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of organic wastewater treatment, and in particular to a method and device for treating organic wastewater by microwave photocatalysis. The method comprises the following steps: a. Using a micro-nano bubble generator to generate micro-nano bubbles in a wastewater treatment device to obtain pretreated wastewater; b. Mixing a composite catalyst with the pretreated wastewater to form a blended system; c. Placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 400-800 W, and maintaining it for 1-8 hours to obtain treated wastewater. The composite catalyst is a carbon-based composite photocatalyst, and its preparation method comprises S1, preparing cellulose-based activated carbon fibers; S2, modifying cellulose-based activated carbon fibers: S3, preparing a carbon-based composite photocatalyst. The present application provides a method and device for treating organic wastewater by microwave photocatalysis to solve the problem that the existing photocatalysts in the related art have a narrow ultraviolet light absorption range and a weak ability to degrade organic pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of organic wastewater treatment, and in particular to a method and device for treating organic wastewater with microwave photocatalysis. Background Art

[0002] Organic wastewater treatment is one of the important links in environmental protection. With the acceleration of industrialization and urbanization, the discharge of organic wastewater increases year by year, and its treatment difficulty also increases day by day.

[0003] In the existing technology, commonly used treatment methods include biological treatment, physical and chemical treatment, and some new treatment technologies, such as advanced oxidation, electrochemical, and photocatalytic oxidation. These new treatment technologies have higher treatment efficiency than traditional treatment methods and are environmentally friendly. Among them, photocatalytic oxidation uses light energy to oxidize organic matter in wastewater into carbon dioxide and water. It has high treatment efficiency, simple operation, low cost, and great application potential.

[0004] In the microwave photocatalytic treatment of organic wastewater, the use of photocatalysts is necessary, and the commonly used photocatalysts mainly include semiconductor materials (such as TiO 2 , ZnO, etc.) and non-metallic catalysts (such as activated carbon, graphene, etc.). Under the irradiation of ultraviolet light or visible light, these catalysts can produce active species such as hydroxyl radicals (·OH) with strong oxidizing properties, thereby oxidizing and decomposing organic matter in wastewater. However, the ultraviolet light absorption range of photocatalysts is relatively narrow, and they are prone to deactivation during long-term use. They have weak ability to degrade organic pollutants and are difficult to meet the treatment needs of large-scale industrial wastewater. Summary of the invention

[0005] The embodiments of the present application provide a method and device for treating organic wastewater by microwave photocatalysis, so as to solve the problem that the existing photocatalysts in the related art have a narrow ultraviolet light absorption range and a weak ability to degrade organic pollutants.

[0006] In a first aspect, a method for treating organic wastewater by microwave photocatalysis is provided, which comprises the following steps:

[0007] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0008] b. Mixing the composite catalyst and the pretreated wastewater in a mass volume ratio of 1:100 to 1:800 to form a blending system;

[0009] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 400-800 W, and maintaining the mixture for 1-8 hours to obtain treated wastewater;

[0010] The composite catalyst is a carbon-based composite photocatalyst, and the preparation method of the carbon-based composite photocatalyst includes:

[0011] S1. preparing cellulose-based activated carbon fibers;

[0012] S2. Modifying the cellulose-based activated carbon fiber:

[0013] The cellulose-based activated carbon fiber is immersed in a modification liquid at a mass ratio of 1:5 to 1:8 at 50 to 60° C. for 2 to 10 hours, filtered, washed with deionized water, and dried to a constant weight to obtain a modified cellulose-based activated carbon fiber;

[0014] S3. Preparation of carbon-based composite photocatalyst:

[0015] S301, Fe 2 O 3 The nanoparticles are dispersed in deionized water at a mass volume ratio of 1:10 to 1:15, and a dispersant is added under continuous stirring. 2 O 3 The mass ratio of nanoparticles is 1:100~1:200, and stirring is continued for 1~3h to obtain Fe 2 O 3 A dispersion, wherein the dispersant is selected from one of sodium lauryl sulfate and sodium pyrophosphate;

[0016] S302, mixing the modified cellulose-based activated carbon fiber with sodium hexametaphosphate, and dispersing them into the Fe 2 O 3 The dispersion is stirred for 3 to 10 hours, and a carbon-based composite photocatalyst is obtained after centrifugal separation, washing and drying. The mass ratio of the sodium hexametaphosphate to the modified cellulose-based activated carbon fiber is 1:20.

[0017] Preferably, after step c, the method further comprises the following steps:

[0018] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and the organic pollutants in the wastewater are degraded under the enhanced microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the free radicals and dissolved oxygen generated.

[0019] Preferably, the modified liquid comprises 1 to 10 parts of ammonium fluoride, 1 to 5 parts of 3-aminopropyltriethoxysilane and 50 parts of deionized water in parts by mass.

[0020] Preferably, the S1 includes:

[0021] S101, pretreatment: washing, drying and crushing the cellulose raw material to obtain a pretreated material;

[0022] S102, cellulose extraction: the pretreated material and the lignin solvent solution are cooked at 60-90°C for 4-8 hours in a mass ratio of 1:10, and the crude cellulose is obtained after filtration, wherein the mass concentration of the lignin solvent solution is 1-5wt%;

[0023] S103, purification and spinning: washing, bleaching, filter pressing and dehydrating, and drying the crude cellulose to obtain fine cellulose, and then spinning the fine cellulose into fibers by wet spinning to obtain spun fibers;

[0024] S104, carbonization: heating the spun fiber to 400-900°C in a nitrogen atmosphere and maintaining the temperature for 4-10 hours to obtain carbonized fiber;

[0025] S105, post-treatment: washing the carbonized fiber with deionized water for several times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0026] Preferably, the lignin solvent is selected from one of sodium sulfite and hydrogen peroxide.

[0027] Preferably, the S3 further includes:

[0028] S303, at 20-30°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fiber of nanoparticles is mixed with 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 10-20min, and then filtered to obtain a solid intermediate product;

[0029] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in deionized water containing micro-nano bubbles at 20-60° C., stirring for 10-30 minutes and then standing for 12-20 hours, and washing with deionized water, filtering, and drying to obtain a carbon-based composite photocatalyst.

[0030] Preferably, in S304, the drying method is vacuum drying, heating to 20-50°C is stopped, and the temperature is kept for 2-4 hours, and the heating rate is 1-5°C / min.

[0031] In a second aspect, a device for a method for treating organic wastewater with microwave photocatalysis is provided, which is used to implement any of the above methods for treating organic wastewater with microwave photocatalysis, and comprises:

[0032] A microwave processing device comprising a microwave generator;

[0033] A wastewater treatment device, which is arranged in the microwave treatment device, and the wastewater treatment device comprises a reaction chamber, in which a stirrer and an ultraviolet light source are arranged, and the stirrer and the ultraviolet light source are connected to a power supply;

[0034] The micro-nano bubble generator is connected with the reaction chamber through a one-way valve.

[0035] The beneficial effects of the technical solution provided by this application include:

[0036] The present application provides a method and device for treating organic wastewater by microwave photocatalysis, wherein the organic wastewater and micro-nano bubbles are placed under microwave light for pretreatment, and the vibration and rotation of water molecules are accelerated by microwave action, thereby increasing the collision frequency between molecules and promoting the decomposition of organic matter. At the same time, the micro-nano bubbles can increase the dissolved oxygen content in the wastewater and promote the oxidation reaction. When the micro-nano bubbles burst in the wastewater, a local high temperature and high pressure environment is generated, which is conducive to the degradation of organic matter.

[0037] At the same time, the present application uses a composite catalyst as a photocatalyst, using cellulose-based activated carbon fiber (CAF), which has oxygen-containing functional groups such as hydroxyl and carboxyl groups and good adsorption capacity, to modify the CAF by introducing fluorine atoms, changing its surface chemical structure, promoting the separation of photogenerated electrons and holes, and improving the photocatalytic performance; and then using Fe 2 O 3 The loading of nanoparticles forms a heterojunction structure, which promotes the separation and migration of photogenerated electrons and holes and effectively improves the photocatalytic efficiency. That is, under microwave radiation, the photocatalytic properties of the modified CAF and the strengthening effect of micro-nano bubbles are utilized to jointly promote the degradation of organic wastewater. The synergistic effect may improve the degradation efficiency. Therefore, it can solve the problem of the narrow ultraviolet light absorption range of existing photocatalysts in related technologies and the weak ability to degrade organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0039] Figure 1A flow chart of the method for treating organic wastewater with microwave photocatalysis provided in this application;

[0040] Figure 2 A flow chart for preparing a carbon-based composite photocatalyst provided in this application;

[0041] Figure 3 A flow chart for preparing cellulose-based activated carbon fibers provided in this application;

[0042] Figure 4 An operation flow chart of the method for treating organic wastewater with microwave photocatalysis provided in this application;

[0043] Figure 5 Schematic diagram of the device for microwave photocatalytic treatment of organic wastewater provided in this application.

[0044] Explanation of the reference numerals: 1. Microwave treatment device; 101. Microwave generator; 2. Wastewater treatment device; 201. Water inlet pipe; 202. Water outlet pipe; 3. Reaction chamber; 301. Agitator; 302. Ultraviolet light source; 4. Micro-nano bubble generator; 401. One-way valve; 5. Power supply. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0046] See also Figure 1~Figure 5 As shown, the present application provides a method for treating organic wastewater by microwave photocatalysis, which comprises the following steps:

[0047] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0048] b. Mixing the composite catalyst and the pretreated wastewater in a mass volume ratio of 1:100 to 1:800 to form a blending system;

[0049] c. Place the blended system in a microwave treatment device, adjust the wavelength of the ultraviolet light source to 180-280 nm, adjust the power of the microwave generator to 400-800 W, and maintain for 1-8 hours to obtain treated wastewater.

[0050] In some embodiments, after step c, the following steps are also included:

[0051] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and the organic pollutants in the wastewater are further degraded under the enhanced microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0052] Specifically, micro-nano bubbles refer to tiny bubbles with a diameter ranging from tens of micrometers to hundreds of nanometers. When the bubble diameter is below 100μm, it is called a micron bubble; and bubbles with a diameter below 100nm are called nanobubbles. Micro-nano bubbles have a series of unique physical and chemical properties, including large specific surface area, slow rising speed, self-pressurized dissolution, surface charge, generation of a large number of free radicals, and high gas dissolution rate.

[0053] After step c, micro-nano bubbles are continuously generated again by the micro-nano bubble generator, and are introduced into the wastewater treatment device to continuously act on the treated wastewater obtained in step c. The organic pollutants in the wastewater are further degraded under the enhanced microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated, thereby improving the degradation capacity of the treatment device for organic matter in the wastewater.

[0054] The composite catalyst is a carbon-based composite photocatalyst, and the preparation method of the carbon-based composite photocatalyst comprises the following steps:

[0055] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0056] S101, pretreatment: washing, drying and crushing the cellulose raw material to obtain a pretreated material;

[0057] S102, cellulose extraction: the pretreated material and the lignin solvent solution are cooked at 60-90°C for 4-8 hours in a mass ratio of 1:10, and the crude cellulose is obtained after filtering, wherein the mass concentration of the lignin solvent solution is 1-5wt%; wherein the lignin solvent is selected from one of sodium sulfite and hydrogen peroxide.

[0058] S103, purification and spinning: washing, bleaching, filter pressing and dehydrating, and drying the crude cellulose to obtain fine cellulose, and then spinning the fine cellulose into fibers by wet spinning or dry spinning technology to obtain spun fibers;

[0059] S104, carbonization: heating the spun fiber to 400-900°C in a nitrogen atmosphere and maintaining the temperature for 4-10 hours to obtain carbonized fiber;

[0060] S105, post-treatment: washing the carbonized fiber with deionized water for several times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0061] S2. Modifying the cellulose-based activated carbon fiber:

[0062] The cellulose-based activated carbon fiber is immersed in a modification liquid at a mass ratio of 1:5-1:8 at 50-60° C. for 2-10 hours, filtered, washed with deionized water, and dried to constant weight to obtain a modified cellulose-based activated carbon fiber.

[0063] In some embodiments, the modified liquid includes 1-10 parts of ammonium fluoride, 1-5 parts of 3-aminopropyltriethoxysilane and 50 parts of deionized water in parts by mass.

[0064] The fluoride salt in the modified solution can introduce fluorine atoms on the surface of CAF and change its surface chemical structure. The introduction of fluorine atoms promotes the separation of photogenerated electrons and holes, reduces the recombination rate of photogenerated carriers, and thus improves the photocatalytic performance of CAF.

[0065] S3. Preparation of carbon-based composite photocatalyst:

[0066] S301, Fe 2 O 3 The nanoparticles are dispersed in deionized water at a mass volume ratio of 1:10 to 1:15, and a dispersant is added under continuous stirring. 2 O 3 The mass ratio of nanoparticles is 1:100~1:200, and stirring is continued for 1~3h to obtain Fe 2 O 3 Dispersion; optionally, the dispersant is selected from one of sodium lauryl sulfate and sodium pyrophosphate.

[0067] The addition of dispersants can effectively increase Fe 2 O 3 Dispersibility in water, and Fe 2 O 3 The heterojunction structure formed between Fe and modified CAF can promote the separation and migration of photogenerated electrons and holes. 2 O 3 and modified CAF absorb light energy and generate electron-hole pairs respectively. Due to the energy level difference between the two, electrons and holes will separate and migrate at the heterojunction interface, thereby reducing the recombination probability of electron-hole pairs; at the same time, it broadens the light absorption range, increases the active sites, provides more reaction opportunities and paths, and effectively improves the photocatalytic efficiency.

[0068] S302, mixing the modified cellulose-based activated carbon fiber with sodium hexametaphosphate, and dispersing them into the Fe 2 O 3The dispersion was stirred for 3-10 hours, and the Fe-loaded 2 O 3 The mass ratio of sodium hexametaphosphate to modified cellulose-based activated carbon fiber is 1:20. Specifically, sodium hexametaphosphate can be adsorbed on the surface of CAF, and its long-chain molecular structure forms a steric hindrance, which hinders the mutual approach and agglomeration of CAF particles, thereby improving the dispersibility and Fe 2 O 3 After the dispersion is mixed, the contact area between the two can be increased, making Fe 2 O 3 Better adsorption on CAF.

[0069] S303, at 20-30°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fiber of nanoparticles is mixed with 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 10-20min, and then filtered to obtain a solid intermediate product;

[0070] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in deionized water containing micro-nano bubbles at 20-60°C, stirring for 10-30min and then standing for 12-20h, washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst. It should be noted that the micro-nano bubble generator in this step can use a JXWNP-L01 low-noise scientific research-grade nano-micro bubble generator, or the micro-nano bubble generator in step a or d. The latter needs to disassemble the micro-nano bubble generator to assist in the preparation of modified cellulose-based activated carbon fibers, but can effectively reduce costs. In the following embodiments, a JXWNP-L01 low-noise scientific research-grade nano-micro bubble generator is used as a micro-nano bubble generator.

[0071] Among them, the drying method in S304 is vacuum drying. After heating to 20~50℃, stop heating and keep warm for 2~4h. The heating rate is 1~5℃ / min.

[0072] Micro-nano bubbles can exist stably in water. Glutaraldehyde is used to load Fe 2 O 3 The nanoparticle CAF is surface treated, and the obtained solid intermediate product is immersed in water containing micro-nano bubbles. The strength of the micro-nano bubbles attached to the CAF surface is enhanced through the cross-linking effect of glutaraldehyde; by fixing the micro-nano bubbles on the surface or in the pores of CAF, the presence of micro-nano bubbles can increase the hydrophilicity and active sites of the CAF surface, thereby facilitating the photocatalytic reaction.

[0073] Example 1

[0074] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0075] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0076] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:200 to form a blending system;

[0077] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 600 W, and maintaining for 4 hours to obtain treated wastewater;

[0078] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 600W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0079] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0080] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0081] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0082] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 5 wt%, and steamed at 80° C. for 6 h, and the crude cellulose was obtained after filtration;

[0083] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0084] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 5 hours to obtain carbonized fiber;

[0085] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0086] S2. Modifying the cellulose-based activated carbon fiber:

[0087] The 30 g cellulose-based activated carbon fiber was immersed in 180 g of the modification liquid at 55° C. for 4 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0088] The modified liquid includes 18 g of ammonium fluoride, 12 g of 3-aminopropyltriethoxysilane and 150 g of deionized water.

[0089] S3. Preparation of carbon-based composite photocatalyst:

[0090] S301, 10g of Fe 2 O 3 The nanoparticles were dispersed in 100 mL of deionized water, and 0.1 g of sodium dodecyl sulfate was added under continuous stirring. The stirring was continued for 2 h to obtain Fe 2 O 3 Dispersion liquid;

[0091] S302, 30g of modified cellulose-based activated carbon fiber and 1.5g of sodium hexametaphosphate were mixed and dispersed into 100g of Fe 2 O 3 The dispersion was stirred for 3 h, and the Fe-loaded 2 O 3 Nanoparticles of cellulose-based activated carbon fibers;

[0092] S303, at 25°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fiber of nanoparticles was mixed with 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 15min, and then filtered to obtain a solid intermediate product;

[0093] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in the deionized water containing micro-nano bubbles at 30° C., stirring for 20 minutes and then standing for 16 hours, and washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst.

[0094] The drying method in S304 is vacuum drying. After heating to 40°C, the heating is stopped and kept warm for 2 hours. The heating rate is 5°C / min.

[0095] Example 2

[0096] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0097] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0098] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:600 ​​to form a blending system;

[0099] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 800 W, and maintaining the mixture for 8 hours to obtain treated wastewater;

[0100] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 800W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0101] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0102] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0103] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0104] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 1 wt%, and steamed at 60° C. for 4 h, and then filtered to obtain a crude cellulose product;

[0105] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0106] S104, carbonization: heating the spun fiber to 400° C. in a nitrogen atmosphere and maintaining the temperature for 10 hours to obtain carbonized fiber;

[0107] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0108] S2. Modifying the cellulose-based activated carbon fiber:

[0109] The 30 g cellulose-based activated carbon fiber was immersed in 150 g of the modification liquid at 50° C. for 4 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0110] The modified liquid includes 12.5 g of ammonium fluoride, 12.5 g of 3-aminopropyltriethoxysilane and 125 g of deionized water.

[0111] S3. Preparation of carbon-based composite photocatalyst:

[0112] S301, 10g of Fe 2 O 3 The nanoparticles were dispersed in 100 mL of deionized water, and 0.05 g of sodium dodecyl sulfate was added under continuous stirring. The stirring was continued for 1 h to obtain Fe 2 O 3 Dispersion liquid;

[0113] S302, 30 g of modified cellulose-based activated carbon fiber and 1.5 g of sodium hexametaphosphate were ultrasonically mixed and dispersed into 90 g of Fe 2 O 3 The dispersion was stirred for 3 h, and the Fe-loaded 2 O 3 Nanoparticles of cellulose-based activated carbon fibers;

[0114] S303, at 25°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fibers of nanoparticles were mixed with 0.5 wt % glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 20 min, and then filtered to obtain a solid intermediate product;

[0115] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in deionized water containing micro-nano bubbles at 20° C., stirring for 30 minutes and then standing for 12 hours, washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst.

[0116] The drying method in S304 is vacuum drying. After heating to 20°C, the heating is stopped and kept warm for 4 hours, with a heating rate of 1°C / min.

[0117] Example 3

[0118] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0119] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0120] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:800 to form a blending system;

[0121] c. Place the blended system in a microwave treatment device, adjust the wavelength of the ultraviolet light source to 180-280 nm, adjust the power of the microwave generator to 600 W, and maintain for 4 hours to obtain treated wastewater.

[0122] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0123] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0124] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0125] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 5 wt%, and steamed at 60° C. for 8 h, and the crude cellulose was obtained after filtration;

[0126] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0127] S104, carbonization: heating the spun fiber to 900° C. in a nitrogen atmosphere and maintaining the temperature for 4 hours to obtain carbonized fiber;

[0128] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0129] S2. Modifying the cellulose-based activated carbon fiber:

[0130] The 60 g cellulose-based activated carbon fiber was immersed in 300 g of the modification liquid at 55° C. for 2 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0131] The modified liquid includes 30 g of ammonium fluoride, 20 g of 3-aminopropyltriethoxysilane and 250 g of deionized water.

[0132] S3. Preparation of carbon-based composite photocatalyst:

[0133] S301, 10g of Fe 2 O 3 The nanoparticles were dispersed in 120 mL of deionized water, and 0.08 g of sodium dodecyl sulfate was added under continuous stirring. The stirring was continued for 2 h to obtain Fe 2 O 3 Dispersion liquid;

[0134] S302, 30g of modified cellulose-based activated carbon fiber and 1.5g of sodium hexametaphosphate were mixed and dispersed into 120g of Fe 2 O 3 The dispersion was stirred for 3 h, and the Fe-loaded 2 O 3 Nanoparticles of cellulose-based activated carbon fibers;

[0135] S303, at 25°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fiber of nanoparticles was mixed with 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 15min, and then filtered to obtain a solid intermediate product;

[0136] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in the deionized water containing micro-nano bubbles at 30° C., stirring for 20 minutes and then standing for 16 hours, and washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst.

[0137] The drying method in S304 is vacuum drying. After heating to 50°C, the heating is stopped and kept warm for 2 hours. The heating rate is 5°C / min.

[0138] Example 4

[0139] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0140] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0141] b. Mixing the composite catalyst and the pretreated wastewater in a mass volume ratio of 1:100 to form a blending system;

[0142] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 400 W, and maintaining for 4 hours to obtain treated wastewater;

[0143] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 400W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0144] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0145] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0146] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0147] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a 3 wt % hydrogen peroxide solution, and steamed at 90° C. for 4 h, and filtered to obtain a crude cellulose product;

[0148] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0149] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 9 hours to obtain carbonized fiber;

[0150] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0151] S2. Modifying the cellulose-based activated carbon fiber:

[0152] The 30 g cellulose-based activated carbon fiber was immersed in 240 g of the modification liquid at 55° C. for 10 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0153] The modified liquid includes 5.4 g of ammonium fluoride, 4.6 g of 3-aminopropyltriethoxysilane and 230 g of deionized water.

[0154] S3. Preparation of carbon-based composite photocatalyst:

[0155] S301, 10g of Fe 2 O 3 The nanoparticles were dispersed in 150 mL of deionized water, and 0.1 g of sodium pyrophosphate was added under continuous stirring. The stirring was continued for 2 h to obtain Fe2 O 3 Dispersion liquid;

[0156] S302, 30g of modified cellulose-based activated carbon fiber and 1.5g of sodium hexametaphosphate were mixed and dispersed into 100g of Fe 2 O 3 The dispersion was stirred for 3 h, and the Fe-loaded 2 O 3 Nanoparticles of cellulose-based activated carbon fibers;

[0157] S303, at 25°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fibers of nanoparticles were mixed with 0.5 wt % glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 20 min, and then filtered to obtain a solid intermediate product;

[0158] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in the deionized water containing micro-nano bubbles at 60° C., stirring for 30 minutes and then standing for 20 hours, and washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst.

[0159] The drying method in S304 is vacuum drying. After heating to 40°C, the heating is stopped and kept warm for 3 hours, with a heating rate of 3°C / min.

[0160] Example 5

[0161] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0162] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0163] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:200 to form a blending system;

[0164] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 600 W, and maintaining for 4 hours to obtain treated wastewater;

[0165] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 600W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0166] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0167] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0168] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0169] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a 3 wt % hydrogen peroxide solution, and steamed at 90° C. for 4 h, and filtered to obtain a crude cellulose product;

[0170] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0171] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 5 hours to obtain carbonized fiber;

[0172] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0173] S2. Modifying the cellulose-based activated carbon fiber:

[0174] The 30 g cellulose-based activated carbon fiber was immersed in 210 g of the modification liquid at 55° C. for 6 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0175] The modified liquid includes 15 g of ammonium fluoride, 7.5 g of 3-aminopropyltriethoxysilane and 187.5 g of deionized water.

[0176] S3. Preparation of carbon-based composite photocatalyst:

[0177] S301, 10g of Fe 2 O 3 The nanoparticles were dispersed in 150 mL of deionized water, and 0.1 g of sodium pyrophosphate was added under continuous stirring. The stirring was continued for 2 h to obtain Fe 2 O 3 Dispersion liquid;

[0178] S302, 30g of modified cellulose-based activated carbon fiber and 1.5g of sodium hexametaphosphate were mixed and dispersed into 100g of Fe 2 O3 The dispersion was stirred for 3 h, and the Fe-loaded 2 O 3 Nanoparticles of cellulose-based activated carbon fibers;

[0179] S303, at 25°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fibers of nanoparticles were mixed with 0.5 wt % glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 20 min, and then filtered to obtain a solid intermediate product;

[0180] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in the deionized water containing micro-nano bubbles at 60° C., stirring for 30 minutes and then standing for 20 hours, and washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst.

[0181] The drying method in S304 is vacuum drying. After heating to 40°C, the heating is stopped and kept warm for 3 hours. The heating rate is 3°C / min.

[0182] Comparative Example 1

[0183] The method for treating organic wastewater by microwave photocatalysis provided in this comparative example comprises the following steps:

[0184] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0185] b. placing the pretreated wastewater in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 600 W, and maintaining the device for 4 hours to obtain treated wastewater;

[0186] c. Use a micro-nano bubble generator to generate micro-nano bubbles in a wastewater treatment device, treat the wastewater treated in step b again, and further degrade it by utilizing the strengthening effect of micro-nano bubbles under 600W microwave radiation.

[0187] Comparative Example 2

[0188] The method for treating organic wastewater by microwave photocatalysis provided in this comparative example comprises the following steps:

[0189] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0190] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:200 to form a blending system;

[0191] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 600 W, and maintaining for 4 hours to obtain treated wastewater;

[0192] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 600W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0193] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0194] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0195] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0196] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 5 wt%, and steamed at 80° C. for 6 h, and the crude cellulose was obtained after filtration;

[0197] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0198] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 5 hours to obtain carbonized fiber;

[0199] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0200] S2. Preparation of carbon-based composite photocatalyst:

[0201] S201, 10g of Fe 2 O 3 The nanoparticles were dispersed in 100 mL of deionized water, and 0.1 g of sodium dodecyl sulfate was added under continuous stirring. The stirring was continued for 2 h to obtain Fe 2 O 3 Dispersion liquid;

[0202] S202, 30g of the cellulose-based activated carbon fiber is mixed with 1.5g of sodium hexametaphosphate and dispersed in 100g of Fe 2 O 3 The dispersion was stirred for 3 h, and the Fe-loaded 2 O 3 Nanoparticles of cellulose-based activated carbon fibers;

[0203] S203, at 25 ° C, the Fe-loaded 2 O 3 The nanoparticle cellulose-based activated carbon fiber was mixed with 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 15 minutes, and then filtered to obtain a solid intermediate product;

[0204] S204, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in deionized water containing micro-nano bubbles at 30° C., stirring for 20 minutes and then standing for 16 hours, and washing with deionized water, filtering, and drying to obtain a carbon-based composite photocatalyst.

[0205] The drying method in this comparative example S204 is vacuum drying. After heating to 40° C., the heating is stopped and kept warm for 2 hours. The heating rate is 5° C. / min.

[0206] Comparative Example 3

[0207] The method for treating organic wastewater by microwave photocatalysis provided in this comparative example comprises the following steps:

[0208] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0209] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:200 to form a blending system;

[0210] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 600 W, and maintaining for 4 hours to obtain treated wastewater;

[0211] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 600W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0212] In the above step b, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0213] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0214] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0215] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 5 wt%, and steamed at 80° C. for 6 h, and the crude cellulose was obtained after filtration;

[0216] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0217] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 5 hours to obtain carbonized fiber;

[0218] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0219] S2. Modifying the cellulose-based activated carbon fiber:

[0220] The 30 g cellulose-based activated carbon fiber was immersed in 180 g of the modification liquid at 55° C. for 4 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0221] The modified liquid includes 18 g of ammonium fluoride, 12 g of 3-aminopropyltriethoxysilane and 150 g of deionized water.

[0222] S3. Preparation of carbon-based composite photocatalyst:

[0223] Micro-nano bubbles were generated in deionized water using a micro-nano bubble generator, the modified cellulose-based activated carbon fiber was immersed in the deionized water containing the micro-nano bubbles at 30° C., stirred for 20 minutes and then allowed to stand for 16 hours, and then washed with deionized water, filtered and dried to obtain a carbon-based composite photocatalyst.

[0224] The drying method in S3 is vacuum drying. After heating to 40°C, the heating is stopped and kept warm for 2 hours, with a heating rate of 5°C / min.

[0225] Comparative Example 4

[0226] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0227] a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater;

[0228] b. Mixing the composite catalyst and the pretreated wastewater at a mass volume ratio of 1:200 to form a blending system;

[0229] c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 600 W, and maintaining for 4 hours to obtain treated wastewater;

[0230] d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater pretreated in step c, and further degrade the wastewater under 600W microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the large amount of free radicals and abundant dissolved oxygen generated.

[0231] In the above step b, the catalyst used is cellulose-based activated carbon fiber. The preparation method of cellulose-based activated carbon fiber in this embodiment includes the following steps:

[0232] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0233] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0234] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 5 wt%, and steamed at 80° C. for 6 h, and the crude cellulose was obtained after filtration;

[0235] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0236] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 5 hours to obtain carbonized fiber;

[0237] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0238] Comparative Example 5

[0239] The method for treating organic wastewater by microwave photocatalysis provided in this embodiment comprises the following steps:

[0240] a. Mixing the composite catalyst and the wastewater to be treated at a mass volume ratio of 1:200 to form a blending system;

[0241] c. Place the blended system in a microwave treatment device, adjust the wavelength of the ultraviolet light source to 180-280 nm, adjust the power of the microwave generator to 600 W, and maintain for 4 hours to obtain treated wastewater.

[0242] In the above step a, the composite catalyst used is a carbon-based composite photocatalyst. The preparation method of the carbon-based composite photocatalyst in this embodiment includes the following steps:

[0243] S1. Preparation of cellulose-based activated carbon fiber (CAF):

[0244] S101, pretreatment: washing, drying and crushing the straw raw material to obtain pretreated material;

[0245] S102, cellulose extraction: 50 g of the pretreated material was mixed with 500 g of a sodium sulfite solution with a mass concentration of 5 wt%, and steamed at 80° C. for 6 h, and the crude cellulose was obtained after filtration;

[0246] S103, purification and spinning: the crude cellulose is washed with deionized water for three times, filtered and dehydrated, and dried to obtain fine cellulose. Then, the fine cellulose is spun into fibers by wet spinning to obtain spun fibers. Specifically, the spinneret hole diameter is 0.05 mm.

[0247] S104, carbonization: heating the spun fiber to 700° C. in a nitrogen atmosphere and maintaining the temperature for 5 hours to obtain carbonized fiber;

[0248] S105, post-treatment: washing the carbonized fiber with deionized water for three times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

[0249] S2. Modifying the cellulose-based activated carbon fiber:

[0250] The 30 g cellulose-based activated carbon fiber was immersed in 180 g of the modification liquid at 55° C. for 4 hours, filtered, washed with deionized water, and dried to constant weight to obtain modified cellulose-based activated carbon fiber.

[0251] The modified liquid includes 18 g of ammonium fluoride, 12 g of 3-aminopropyltriethoxysilane and 150 g of deionized water.

[0252] S3. Preparation of carbon-based composite photocatalyst:

[0253] S301, 10g of Fe 2 O 3 The nanoparticles were dispersed in 100 mL of deionized water, and 0.1 g of sodium dodecyl sulfate was added under continuous stirring. The stirring was continued for 2 h to obtain Fe 2 O 3 Dispersion liquid;

[0254] S302, 30g of modified cellulose-based activated carbon fiber and 1.5g of sodium hexametaphosphate were mixed and dispersed into 100g of Fe 2 O 3 The dispersion was stirred for 3 hours, and the carbon-based composite photocatalyst was obtained after centrifugal separation, washing and drying.

[0255] S303, at 25°C, the Fe-loaded 2 O 3 The modified cellulose-based activated carbon fiber of nanoparticles was mixed with 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirred for 15min, and then filtered to obtain a solid intermediate product;

[0256] S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in the deionized water containing micro-nano bubbles at 30° C., stirring for 20 minutes and then standing for 16 hours, and washing with deionized water, filtering and drying to obtain a carbon-based composite photocatalyst.

[0257] The drying method in S304 is vacuum drying. After heating to 40°C, the heating is stopped and kept warm for 2 hours. The heating rate is 5°C / min.

[0258] Specifically, the comparison of the preparation methods of the carbon-based composite photocatalysts in Examples 1 to 5 and the amount of the modified liquid added are shown in Table 1.

[0259] Table 1 Preparation method of carbon-based composite photocatalyst and amount of modified liquid added in Examples 1 to 5

[0260]

[0261] In Comparative Examples 1 to 5, the comparison of the provided methods for treating organic wastewater with microwave photocatalysis and the methods for preparing carbon-based composite photocatalysts is shown in Table 2.

[0262] Table 2 Wastewater treatment methods and carbon-based composite photocatalyst preparation methods in Comparative Examples 1 to 5

[0263]

[0264] Taking rhodamine B as the target pollutant, the carbon-based composite photocatalysts prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were used to treat organic wastewater with microwave photocatalysis.

[0265] Specifically, 10L of organic wastewater is provided, wherein the initial concentration of Rhodamine B in the organic wastewater is 20mg / L, and the carbon-based composite photocatalyst is added according to the addition ratio of Examples 1 to 5 and Comparative Examples 1 to 5, mixed and stirred, reacted at room temperature 25 to 27°C, and wastewater samples are taken at 1h, 2h, 4h and 8h to detect the concentration of Rhodamine B therein, and the removal rate is calculated. The removal rate test results are shown in Table 3. The mass volume ratio in Table 3 is the mass volume ratio of the carbon-based composite photocatalyst to the organic wastewater.

[0266] Table 3 Removal of Rhodamine B from wastewater by Examples 1 to 5 and Comparative Examples 1 to 5

[0267]

[0268] It can be seen that the methods provided in Examples 1 and 4 of the present application and the carbon-based composite photocatalysts used therein have a high removal efficiency. This is because the high adsorption of cellulose-based activated carbon fibers helps to enrich organic pollutants on the catalyst surface. The modified cellulose-based activated carbon fibers, on the one hand, introduce fluorine atoms to change their surface chemical structure, promote the separation of photogenerated electrons and holes, and improve the photocatalytic performance. On the other hand, they increase the active sites and load Fe 2 O 3 Nanoparticles form a heterojunction structure, which promotes the separation and migration of photogenerated electrons and holes, effectively improving the photocatalytic efficiency. Then, micro-nano bubbles are used to coat Fe 2 O 3 The modified CAF of nanoparticles and the high adsorption of the modified CAF help to enrich the organic pollutants on the catalyst surface, while the hydroxyl radical generation ability of the micro-nano bubbles helps to accelerate the oxidative decomposition of organic matter, thereby achieving a more efficient degradation of organic pollutants. The micro-nano bubbles can also enhance the scattering and absorption of light and improve the light utilization rate of the photocatalytic reaction. In the preferred method for treating organic wastewater of the present application (Example 1), the removal rate of organic matter in the organic wastewater can reach more than 98%.

[0269] The present application also provides a microwave photocatalytic treatment device for organic wastewater, see Figure 5As shown, the treatment device includes a microwave treatment device 1, a wastewater treatment device 2 and a micro-nano bubble generator 4, wherein the microwave treatment device 1 includes a microwave generator 101, the wastewater treatment device 2 includes a reaction chamber 3, in which an agitator 301 and an ultraviolet light source 302 are arranged, and the wastewater treatment device 2 includes a water inlet pipe 201 and a water outlet pipe 202, and the water inlet pipe 201 and the water outlet pipe 202 are both connected to the reaction chamber 3.

[0270] Further, the agitator 301, the ultraviolet light source 302 and the microwave generator 101 are connected to the power supply 5, and the micro-nano bubble generator 4 is connected to the reaction chamber 3 through the one-way valve 401, and the micro-nano bubble generator 4 is connected to the power supply 5. When the reaction chamber 3 is equipped with wastewater to be treated, the one-way valve 401 is opened, the micro-nano bubble generator 4 generates micro-nano bubbles, and transports them to the reaction chamber 3, and the power supply 5 controls the agitator 301, the ultraviolet light source 302, and the microwave generator 101 to be opened, so that the micro-nano bubbles are mixed with the wastewater to achieve pretreatment. When the processing step proceeds to b, that is, after the composite catalyst is put into the power supply 5, the agitator 301 and the ultraviolet light source 302 are continuously operated, and the one-way valve 401 is closed, so that the blending system is degraded under microwave radiation and ultraviolet light irradiation.

[0271] Optionally, combined Figure 2 As shown, the microwave generator 101 is arranged on the inner wall of the microwave processing device 1 .

[0272] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for treating organic wastewater by microwave photocatalysis, characterized in that: It includes the following steps: a. Providing a wastewater treatment device and a micro-nano bubble generator, and using the micro-nano bubble generator to generate micro-nano bubbles in the wastewater treatment device to obtain pretreated wastewater; b. Mixing and stirring the composite catalyst and the pretreated wastewater in a mass volume ratio of 1:100 to 1:800 to form a blending system, wherein the unit of the mass volume ratio is g:L; c. placing the blended system in a microwave treatment device, adjusting the wavelength of the ultraviolet light source to 180-280 nm, adjusting the power of the microwave generator to 400-800 W, and maintaining the mixture for 1-8 hours to obtain treated wastewater; d. The micro-nano bubbles continuously generated by the micro-nano bubble generator continuously act on the wastewater treated in step c, and the organic pollutants in the wastewater are degraded under the enhanced microwave radiation by utilizing the charges on the surface of the micro-nano bubbles and the free radicals and dissolved oxygen generated; The composite catalyst is a carbon-based composite photocatalyst, and the preparation method of the carbon-based composite photocatalyst includes: S1, preparing cellulose-based activated carbon fibers; S2. Modifying the cellulose-based activated carbon fiber: The cellulose-based activated carbon fiber is immersed in a modification liquid at a mass ratio of 1:5 to 1:8 at 50 to 60° C. for 2 to 10 hours, filtered, washed with deionized water, and dried to a constant weight to obtain a modified cellulose-based activated carbon fiber; In terms of mass fractions, the modified liquid is composed of 1 to 10 parts of ammonium fluoride, 1 to 5 parts of 3-aminopropyltriethoxysilane and 50 parts of deionized water; S3. Preparation of carbon-based composite photocatalyst: S301, dispersing Fe2O3 nanoparticles in deionized water at a mass volume ratio of 1:10-1:15, adding a dispersant under continuous stirring, wherein the mass ratio of the dispersant to the Fe2O3 nanoparticles is 1:100-1:200, and continuing stirring for 1-3 hours to obtain a Fe2O3 dispersion, wherein the dispersant is selected from one of sodium dodecyl sulfate and sodium pyrophosphate, and the unit of the mass volume ratio is g:mL; S302, after mixing the modified cellulose-based activated carbon fiber with sodium hexametaphosphate, disperse the mixture of the modified cellulose-based activated carbon fiber and sodium hexametaphosphate into the Fe2O3 dispersion at a mass ratio of 1:3 to 1:4, stir for 3 to 10 hours, and obtain cellulose-based activated carbon fibers loaded with Fe2O3 nanoparticles after centrifugal separation, washing, and drying, wherein the mass ratio of sodium hexametaphosphate to the modified cellulose-based activated carbon fiber is 1:20; S303, at 20-30° C., mixing the cellulose-based activated carbon fiber loaded with Fe2O3 nanoparticles prepared in S302 with a 0.5wt% glutaraldehyde solution in a mass volume ratio of 1:10 and stirring for 10-20 minutes, filtering to obtain a solid intermediate product, wherein the unit of the mass volume ratio is g:mL; S304, using a micro-nano bubble generator to generate micro-nano bubbles in deionized water, immersing the solid intermediate product in deionized water containing micro-nano bubbles at 20-60° C., stirring for 10-30 minutes and then standing for 12-20 hours, and washing with deionized water, filtering, and drying to obtain a carbon-based composite photocatalyst.

2. The method for treating organic wastewater by microwave photocatalysis according to claim 1, characterized in that: The S1 includes: S101, pretreatment: washing, drying and crushing the cellulose raw material to obtain a pretreated material; S102, cellulose extraction: the pretreated material and the lignin solvent solution are cooked at 60-90°C for 4-8 hours in a mass ratio of 1:10, and the crude cellulose is obtained after filtration, wherein the mass concentration of the lignin solvent solution is 1-5wt%; S103, purification and spinning: washing, bleaching, filter pressing and dehydrating, and drying the crude cellulose to obtain fine cellulose, and then spinning the fine cellulose into fibers by wet spinning to obtain spun fibers; S104, carbonization: heating the spun fiber to 400-900°C in a nitrogen atmosphere and maintaining the temperature for 4-10 hours to obtain carbonized fiber; S105, post-treatment: washing the carbonized fiber with deionized water for several times, drying to a constant weight after centrifugation to obtain cellulose-based activated carbon fiber.

3. The method for treating organic wastewater by microwave photocatalysis according to claim 2, characterized in that: The lignin solvent is selected from one of sodium sulfite and hydrogen peroxide.

4. The method for treating organic wastewater by microwave photocatalysis according to claim 1, characterized in that: In the S304, the drying method is vacuum drying, heating to 20-50°C and then stopping heating, keeping the temperature for 2-4 hours, and the heating rate is 1-5°C / min.