A magnesium slag modified coal gangue-based composite backfill material, its preparation method and application

By modifying magnesium slag and activating coal gangue with water glass, a magnesium slag-modified coal gangue-based composite backfill material was prepared, which solved the problems of poor cementitious properties and long setting time in the existing technology, and realized the preparation of high-strength, low-cost backfill material and environmentally friendly waste disposal.

CN118652081BActive Publication Date: 2026-11-10XIAN RES INST OF CHINA COAL TECH & ENG GRP CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410631290.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2026-11-10
Estimated Expiration
2044-05-21

AI Technical Summary

Technical Problem

Existing coal gangue and magnesium slag backfill materials have poor cementitious properties, long setting time, and low strength. Furthermore, directly mixed slurries do not possess cementitious properties, which may cause environmental hazards.

Method used

Magnesium slag was modified by dissolving carbon dioxide in water to form a carbonate solution, which transformed the free calcium-containing phase in the magnesium slag into calcium carbonate particles. Combined with water glass to excite coal gangue, a magnesium slag-modified coal gangue-based composite backfill material was prepared. The performance was adjusted by controlling the ratio of components A and B.

Benefits of technology

It improves the stability of cementitious materials, shortens the setting time, enhances the strength of filling materials, reduces preparation costs, and achieves the synergistic treatment of magnesium slag and coal gangue, avoiding the risk of blockage during grouting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652081B_ABST
    Figure CN118652081B_ABST
Patent Text Reader

Abstract

This invention provides a magnesium slag-modified coal gangue-based composite backfill material, its preparation method, and its application. The preparation method includes: classifying and crushing coal gangue to obtain coal gangue aggregate and coal gangue active powder; crushing and grinding magnesium slag to obtain magnesium slag active powder; mixing the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stirring evenly to obtain component A; mixing the prescribed amounts of magnesium slag active powder and saturated carbonic acid solution to obtain a slurry; continuously introducing compressed carbon dioxide into the slurry under stirring conditions, and stirring evenly to obtain component B; and mixing component A and component B slurries evenly at a mass ratio of 1:(0.5-1). Component A includes the following raw material components: water glass, coal gangue aggregate, coal gangue active powder, and water; component B includes magnesium slag active powder, saturated carbonic acid solution, and carbon dioxide. This invention improves the stability of the cementitious material and can absorb a large amount of carbon dioxide gas, providing a new means for carbon emission reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of mining materials and relates to composite filling materials, specifically to a magnesium slag modified coal gangue-based composite filling material, its preparation method, and its application. Background Technology

[0002] Both coal mining and the Pidgeon process for magnesium production generate large amounts of solid waste, with coal gangue and magnesium slag being the two most significant types. Long-term stockpiling of these solid wastes not only occupies land but also causes irreparable damage to the ecological environment. Currently, coal gangue and magnesium slag are mainly used for building materials or as direct backfill in mined-out areas. The production of building materials primarily utilizes the abundant calcium, silicon, and aluminum elements in these materials. After mechanical and chemical activation, they can be combined with cement to form a cementitious material. However, a drawback is that the coal gangue requires high-temperature processing before use. Calcination at low temperature is problematic, but excessive calcium-containing phases in magnesium slag can affect the stability of cementitious materials. Direct filling involves grinding coal gangue and magnesium slag into powder, mixing it with water to form a slurry, and then directly filling it into underground spaces. However, this method has drawbacks: the directly mixed slurry lacks cementitious properties, the filling material has a long setting time, low strength, high cost, and difficulty in solidifying the harmful elements contained in the solid waste, which may cause environmental hazards. Therefore, finding a new method for the co-processing of coal gangue and magnesium slag is of great significance for the sustainable development of coal mines and the magnesium industry. Summary of the Invention

[0003] In view of the defects and deficiencies of the existing technology, the purpose of this invention is to provide a magnesium slag modified coal gangue-based composite backfill material, its preparation method and application, so as to solve the technical problems of poor cementitious properties, long setting time and low strength of the backfill material in the existing technology.

[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0005] A method for preparing a magnesium slag modified coal gangue-based composite backfill material includes the following steps: Step 1: Crush and grind coal gangue to obtain coal gangue aggregate and coal gangue active powder; crush and grind magnesium slag to obtain magnesium slag active powder; Step 2: Mix the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stir until homogeneous to obtain component A; Step 3: Mix the magnesium slag active powder and saturated carbonic acid solution according to the formula to obtain a slurry. Under stirring conditions, continuously introduce compressed carbon dioxide into the slurry and stir evenly to obtain component B. Step 4: Mix component A and component B slurry evenly at a mass ratio of 1:(0.5~1) to obtain the final product; The A component, by mass percentage, comprises the following raw material components: water glass 16.9~20.2%, coal gangue aggregate 48.2~54.7%, coal gangue active powder 14.1~18.4%, and water 9.3~13.8%, with the total mass percentage of each component being 100%. Component B, by mass percentage, comprises the following raw material components: 30.8-42.7% magnesium slag active powder, 48.8-56.9% saturated carbonic acid solution, and 8.5-12.3% carbon dioxide, with the total mass percentage of each component being 100%.

[0006] The present invention also has the following technical features: Specifically, the coal gangue aggregate has a particle size greater than 100 mesh, the coal gangue active powder has a particle size less than 100 mesh, and the magnesium slag active powder has a particle size less than 100 mesh.

[0007] Furthermore, the stirring rate in step 2 is 120~140 r / min.

[0008] Furthermore, the stirring rate in step 3 is 220~240 r / min.

[0009] Furthermore, the preparation method specifically includes the following steps: Step 1: Crush and grind coal gangue to obtain coal gangue aggregate with a particle size greater than 100 mesh and coal gangue active powder with a particle size less than 100 mesh; crush and grind magnesium slag to obtain magnesium slag active powder with a particle size less than 100 mesh. Step 2: Mix the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stir until homogeneous to obtain component A; Step 3: Mix the magnesium slag active powder and saturated carbonic acid solution according to the formula to obtain a slurry. Under stirring conditions, continuously introduce compressed carbon dioxide into the slurry and stir evenly to obtain component B. Step 4: Mix component A and component B slurry evenly at a mass ratio of 1:1 to obtain the final product. Component A, by mass percentage, comprises the following raw material components: water glass 17.9%, coal gangue aggregate 53.7%, coal gangue active powder 14.8%, and water 13.6%. The B component, by mass percentage, consists of 41.7% magnesium slag active powder, 49.5% saturated carbonic acid solution, and 8.8% carbon dioxide.

[0010] This invention also protects a magnesium slag modified coal gangue-based composite backfill material, which is prepared by the method described above for preparing magnesium slag modified coal gangue-based composite backfill material.

[0011] Furthermore, the total content of CaO and MgO in the magnesium slag is greater than 70% of the total mass of the magnesium slag, and the loss on ignition of both the coal gangue aggregate and the coal gangue active powder is less than 20%.

[0012] Furthermore, the compressive strength of the magnesium slag modified coal gangue-based composite backfill material is 3~10MPa, the initial setting time is 20~30min, and the final setting time is 2~3h.

[0013] This invention also protects the application of the magnesium slag modified coal gangue-based composite backfill material as described above for backfilling goaf areas.

[0014] Compared with the prior art, the present invention has the following beneficial technical effects: (I) The method of the present invention utilizes carbon dioxide dissolved in water to form a carbonate solution to modify magnesium slag. This not only converts the free calcium (magnesium) phase in the magnesium slag into calcium carbonate particles, reduces the activity of calcium-containing substances, and improves the stability of cementitious materials, but also absorbs a large amount of carbon dioxide greenhouse gas, providing a new technical means for carbon emission reduction. The method of the present invention utilizes modified magnesium slag and water glass to composite-activate coal gangue, which not only makes up for the lack of calcium-containing phase in coal gangue and accelerates the initial and final setting of cementitious materials, but also synergistically disposes of a large amount of magnesium slag and coal gangue.

[0015] (II) The magnesium slag modified coal gangue-based composite backfill material provided by the present invention has cementitious properties. The performance of the backfill material can be controlled by adjusting the ratio of components A and B according to different backfilling requirements. At the same time, neither component has cementitious properties before mixing, which can effectively avoid the risk of blockage during the grouting process. Attached Figure Description

[0016] Figure 1 The preparation process of the magnesium slag modified coal gangue-based composite backfill material in Example 1 is as follows; Figure 2 This is a microstructure diagram of the magnesium slag modified coal gangue-based composite backfill material prepared in Example 1.

[0017] The technical solution of the present invention will be further described below with reference to the embodiments. Detailed Implementation

[0018] It should be noted that, unless otherwise specified, all raw materials and testing methods used in this invention are those known in the art.

[0019] The test method for setting time of materials is based on the "Test Method for Standard Consistency Water Requirement, Setting Time and Soundness of Cement" (GB / T1346-2011); the test method for compressive strength is based on the "Standard Test Method for Physical and Mechanical Properties of Concrete" (GB / T50081-2019); and the test method for curing rate of harmful elements is based on the "Horizontal Oscillation Method for Leaching Toxicity of Solid Waste" published in April 2010.

[0020] The yield of CASH, MASH, NASH mixed gels and calcium carbonate was determined by XRD-Retive spectral analysis, which directly yielded the specific mass percentage of all crystals in the sample. The mixed gel content was obtained by subtracting the percentage of all crystals from the mixture content.

[0021] The technical concept of this invention is as follows: Magnesium slag is modified using a carbonated solution formed by dissolving carbon dioxide in water. This transforms the free calcium (magnesium) phase in the magnesium slag into calcium carbonate particles, reducing the activity of the calcium-containing substances and improving the stability of the cementitious material. Simultaneously, it absorbs a large amount of carbon dioxide greenhouse gas. The modified magnesium slag and water glass are then used to activate coal gangue, dissolving the silica-alumina phase in the coal gangue to form CASH / MASH / NASH gel. This provides the material with cementitious properties and compensates for the lack of calcium-containing phases in the coal gangue, accelerating the initial and final setting of the cementitious material and achieving the synergistic treatment of large quantities of magnesium slag and coal gangue.

[0022] This invention provides a method for preparing a magnesium slag-modified coal gangue-based composite backfill material, comprising the following steps: Step 1: Crush and grind coal gangue to obtain coal gangue aggregate and coal gangue active powder; crush and grind magnesium slag to obtain magnesium slag active powder; The coal gangue aggregate has a particle size greater than 100 mesh, the coal gangue active powder has a particle size less than 100 mesh, and the magnesium slag active powder has a particle size less than 100 mesh.

[0023] Step 2: Mix the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stir until homogeneous to obtain component A; wherein the stirring speed is 120~140 r / min.

[0024] Given that the primary purpose of the backfilling process is still to dispose of coal gangue at a low cost, as much coal gangue as possible should be added while ensuring the strength and setting time of the backfilling material. Coal gangue aggregate has a relatively low preparation cost. Under the above gradation conditions, the cementitious material fills the gaps between the aggregates and binds the aggregates to form a stable structure. In addition, using low-cost coal gangue aggregate and coal gangue active powder as the main body of the backfilling material greatly increases the proportion of coal gangue in the material and reduces the preparation cost of the backfilling material.

[0025] Step 3: Mix the magnesium slag active powder and saturated carbonic acid solution according to the formula to obtain a slurry. Under stirring conditions, continuously introduce compressed carbon dioxide into the slurry and stir until uniform to obtain component B. The stirring rate is 220~240 r / min.

[0026] Step 4: Mix component A and component B slurry evenly at a mass ratio of 1:(0.5~1) to obtain the final product; The A component, by mass percentage, comprises the following raw material components: water glass 16.9~20.2%, coal gangue aggregate 48.2~54.7%, coal gangue active powder 14.1~18.4%, and water 9.3~13.8%, with the total mass percentage of each component being 100%. Component B, by mass percentage, comprises the following raw material components: 30.8-42.7% magnesium slag active powder, 48.8-56.9% saturated carbonic acid solution, and 8.5-12.3% carbon dioxide, with the total mass percentage of each component being 100%.

[0027] The magnesium slag-modified coal gangue-based composite backfill material prepared by this invention has a main hydration product of CASH / MASH / NASH mixed gel, and the formation mechanism of the gel is shown in the following reaction formula: (1) (2) + CASH / MASH / NASH (3) As can be seen from the above expression, the preparation method provided by the present invention can remove calcium magnesium silicate compounds (MgSiO2) from magnesium slag. ) is transformed into calcium carbonate or magnesium carbonate and active silica ( In this mixture, calcium carbonate or magnesium carbonate is suspended in the solution as fine particles, which can be effectively deposited on the surface of the mixed gel to enhance the mechanical properties of the filling material. In reaction (1), carbonic acid is provided by carbon dioxide dissolved in water (reaction (2)). When components A and B are mixed, the unreacted components in the solution... Dissolved from component A And the active silicic acid obtained from component B ( The two react together to form a mixed gel, which provides strength to the filling material. Following the above technical solutions, specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent modifications made based on the technical solutions of this application fall within the protection scope of the present invention.

[0028] Example 1 Following the above technical solutions, such as Figure 1 As shown in the figure, this embodiment provides a method for preparing a magnesium slag modified coal gangue-based composite backfill material, which includes the following steps: Step 1: Crush and grind coal gangue to obtain coal gangue aggregate with a particle size greater than 100 mesh and coal gangue active powder with a particle size less than 100 mesh; crush and grind magnesium slag to obtain magnesium slag active powder with a particle size less than 100 mesh. Step 2: Mix the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stir until homogeneous to obtain component A; the stirring rate is 120 r / min.

[0029] Step 3: Mix the magnesium slag active powder and saturated carbonic acid solution according to the formula to obtain a slurry. Under stirring conditions, continuously introduce compressed carbon dioxide into the slurry and stir until uniform to obtain component B. The stirring rate is 240 r / min.

[0030] Step 4: Mix component A and component B slurry evenly at a mass ratio of 1:1 to obtain the final product. Component A, by mass percentage, comprises the following raw material components: 20.2% water glass, 48.2% coal gangue aggregate, 18.4% coal gangue active powder, and 13.2% water; The B component, by mass percentage, consists of 40.2% magnesium slag active powder, 49.3% saturated carbonic acid solution, and 10.5% carbon dioxide.

[0031] This embodiment ultimately yielded a magnesium slag-modified coal gangue-based composite backfill material.

[0032] The 28-day microstructure of the magnesium slag modified coal gangue-based composite backfill material prepared in this embodiment is as follows: Figure 2 As shown in the figure, it can be seen that all components of the raw materials have reacted fully. The left side is the flocculent gel generated by the reaction, and the right side is the coal gangue aggregate. It can be seen that the generated gel and aggregate are tightly bonded. This dense microstructure provides the material with strong mechanical properties.

[0033] In this embodiment, a portion of the prepared products were selected to make samples, and then the setting time, 7-day compressive strength, 28-day compressive strength, and yield of CASH, MASH, and NASH mixed gels were tested. The test results are shown in Table 1.

[0034] Example 2 This embodiment provides a method for preparing a magnesium slag modified coal gangue-based composite backfill material. The raw material components and preparation steps used in the preparation method are the same as those in Example 1, except that the content of water glass in component A is reduced. Component A, by mass percentage, includes the following raw material components: water glass 18.5%, coal gangue 52.4%, coal gangue active powder 17.9%, and water 12.2%.

[0035] This embodiment ultimately yielded a magnesium slag-modified coal gangue-based composite backfill material.

[0036] In this embodiment, a portion of the prepared products were selected to make samples, and then the setting time, 7-day compressive strength, 28-day compressive strength, and yield of CASH, MASH, and NASH mixed gels were tested. The test results are shown in Table 1.

[0037] Example 3 This embodiment provides a method for preparing a magnesium slag modified coal gangue-based composite backfill material. The raw material components and preparation steps used in the preparation method are the same as those in Example 1. The main difference is that the content of water glass in component A is reduced. Component A, by mass percentage, includes the following raw material components: water glass 17.1%, coal gangue 53.9%, coal gangue active powder 16.7%, and water 12.3%.

[0038] This embodiment ultimately yielded a magnesium slag-modified coal gangue-based composite backfill material.

[0039] In this embodiment, a portion of the prepared products were selected to make samples, and then the setting time, 7-day compressive strength, 28-day compressive strength, and yield of CASH, MASH, and NASH mixed gels were tested. The test results are shown in Table 1.

[0040] Example 4 This embodiment provides a method for preparing a magnesium slag modified coal gangue-based composite backfill material. The raw material components and preparation steps used in the preparation method are the same as those in Example 1. The difference is that the content of magnesium slag active powder in component B is reduced. Component B, by mass percentage, includes the following raw material components: 36.9% magnesium slag active powder, 52.4% saturated carbonic acid solution, and 10.7% carbon dioxide.

[0041] In this embodiment, a portion of the prepared products were selected to make samples, and then the setting time, 7-day compressive strength, 28-day compressive strength, and yield of CASH, MASH, and NASH mixed gels were tested. The test results are shown in Table 1.

[0042] Example 5 This embodiment provides a method for preparing a magnesium slag modified coal gangue-based composite backfill material. The raw material components and preparation steps used in the preparation method are the same as those in Example 1. The difference is that the content of magnesium slag active powder in component B is reduced. Component B, by mass percentage, includes the following raw material components: 31.7% magnesium slag active powder, 56.6% saturated carbonic acid solution, and 11.7% carbon dioxide.

[0043] In this embodiment, a portion of the prepared products were selected to make samples, and then the setting time, 7-day compressive strength, 28-day compressive strength, and yield of CASH, MASH, and NASH mixed gels were tested. The test results are shown in Table 1.

[0044]

[0045] Table 1. Performance test results of the composite filling materials prepared in Examples 1 to 5 Comparative Example 1 This comparative example provides a method for activating coal gangue with only magnesium slag and preparing filling material. The raw material components and preparation steps used in the preparation method are the same as those in Example 1. The difference is that water glass is not added to component A. The raw material components include: 63.9% coal gangue, 23.8% coal gangue active powder, and 12.3% water.

[0046] In this embodiment, a portion of the prepared products were selected to make samples, and then the setting time, 7-day compressive strength, 28-day compressive strength, and yield of CASH, MASH, and NASH mixed gels were tested. The test results are shown in Table 1.

[0047] Comparative Example 2 This embodiment provides a method for activating coal gangue with water glass and preparing filling material. The raw material components and preparation steps used in the preparation method are the same as those in Example 1. The difference is that magnesium slag active powder is not used in component B. That is, component B includes the following raw material components by mass percentage: 79.6% saturated carbonic acid solution and 20.4% carbon dioxide.

[0048] From Examples 1 to 5, and Comparative Examples 1 and 2, it can be seen that: The 7-day and 28-day compressive strengths of the composite backfill material are both related to the amount of magnesium slag and water glass added to the raw materials. The higher the proportion of magnesium slag and water glass, the higher the compressive strength and the shorter the setting time of the material. This indicates that the addition of magnesium slag and water glass plays a decisive role in the activation of coal gangue. The strength of the backfill materials obtained in Comparative Examples 1 and 2 decreased significantly, and the setting time increased significantly. This is not much different from the performance of conventional backfill materials and cannot achieve rapid hardening and early strength of the material. Therefore, the two-component synergistic activation technology described in this invention is more practical.

[0049] Because the raw materials used in this invention are rich in a large amount of The presence of active silica results in rapid gel formation and short setting time during preparation. Therefore, components A and B need to be prepared separately during the filling process. These two slurries are then pumped separately to the vicinity of the filling area and thoroughly mixed in a mixer before being injected into the goaf to prevent clogging during grouting.

[0050] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.

[0051] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0052] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A method for preparing a magnesium slag modified coal gangue-based composite backfill material, characterized in that, Includes the following steps: Step 1: Crush and grind coal gangue to obtain coal gangue aggregate and coal gangue active powder; crush and grind magnesium slag to obtain magnesium slag active powder; Step 2: Mix the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stir until homogeneous to obtain component A; Step 3: Mix the magnesium slag active powder and saturated carbonic acid solution according to the formula to obtain a slurry. Under stirring conditions, continuously introduce compressed carbon dioxide into the slurry and stir evenly to obtain component B. Step 4: Mix component A and component B slurry at a mass ratio of 1:(0.5~1) until homogeneous to obtain the final product; The A component, by mass percentage, comprises the following raw material components: water glass 16.9~20.2%, coal gangue aggregate 48.2~54.7%, coal gangue active powder 14.1~18.4%, and water 9.3~13.8%, with the total mass percentage of each component being 100%. Component B, by mass percentage, comprises the following raw material components: 30.8-42.7% magnesium slag active powder, 48.8-56.9% saturated carbonic acid solution, and 8.5-12.3% carbon dioxide, with the total mass percentage of each component being 100%.

2. The preparation method of the magnesium slag modified coal gangue-based composite backfill material as described in claim 1, characterized in that, The coal gangue aggregate has a particle size greater than 100 mesh, the coal gangue active powder has a particle size less than 100 mesh, and the magnesium slag active powder has a particle size less than 100 mesh.

3. The preparation method of the magnesium slag modified coal gangue-based composite backfill material as described in claim 1, characterized in that, The stirring speed in step 2 is 120~140 r / min.

4. The preparation method of the magnesium slag modified coal gangue-based composite backfill material as described in claim 1, characterized in that, The stirring speed in step 3 is 220~240 r / min.

5. The preparation method of the magnesium slag modified coal gangue-based composite backfill material as described in claim 1, characterized in that, The preparation method specifically includes the following steps: Step 1: Crush and grind coal gangue to obtain coal gangue aggregate with a particle size greater than 100 mesh and coal gangue active powder with a particle size less than 100 mesh; crush and grind magnesium slag to obtain magnesium slag active powder with a particle size less than 100 mesh. Step 2: Mix the prescribed amounts of coal gangue aggregate, coal gangue active powder, water glass, and water, and stir until homogeneous to obtain component A; Step 3: Mix the magnesium slag active powder and saturated carbonic acid solution according to the formula to obtain a slurry. Under stirring conditions, continuously introduce compressed carbon dioxide into the slurry and stir evenly to obtain component B. Step 4: Mix component A and component B slurry evenly at a mass ratio of 1:1 to obtain the final product. Component A, by mass percentage, comprises the following raw material components: water glass 17.9%, coal gangue aggregate 53.7%, coal gangue active powder 14.8%, and water 13.6%. The B component, by mass percentage, consists of 41.7% magnesium slag active powder, 49.5% saturated carbonic acid solution, and 8.8% carbon dioxide.

6. A magnesium slag modified coal gangue-based composite backfill material, characterized in that, The composite backfill material is prepared using the preparation method of magnesium slag modified coal gangue-based composite backfill material as described in any one of claims 1 to 5.

7. The magnesium slag modified coal gangue-based composite backfill material as described in claim 6, characterized in that, The total content of CaO and MgO in the magnesium slag is greater than 70% of the total mass of the magnesium slag, and the loss on ignition of both the coal gangue aggregate and the coal gangue active powder is less than 20%.

8. The magnesium slag modified coal gangue-based composite backfill material as described in claim 6, characterized in that, The compressive strength of the magnesium slag modified coal gangue-based composite backfill material is 3~10MPa, the initial setting time is 20~30min, and the final setting time is 2~3h.

9. The application of the magnesium slag modified coal gangue-based composite backfill material as described in any one of claims 6 to 8 for backfilling goaf areas.

Citation Information

Patent Citations

  • Coal gangue-based composite geopolymer grouting filling material and preparation method thereof

    CN111018423A

  • Method for preparing calcium carbonate binder through CO2 activation

    CN116199525A