A method for preparing a back-contact battery with reduced risk of grid line short circuit and a back-contact battery
By etching and printing insulating blocks on the back of the silicon wafer, combined with plasma defoaming treatment, the problem of local short circuit in the preparation of back contact battery is solved, and the efficiency and insulation effect of the battery are improved.
Patent Information
- Application Number
- CN202411140287.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing back contact battery preparation process can easily lead to local short circuits, resulting in a decrease in battery efficiency.
Grooves are etched on the back of the silicon wafer to form grooves, and insulating blocks and metal electrodes are printed on the grooves, followed by plasma defoaming to prevent silver paste from penetrating the insulating blocks and fine gate connections and reducing the risk of short circuits.
It effectively reduces the risk of gate line short circuit and improves battery efficiency and insulation effect.
Smart Images

Figure CN118658901B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of back-contact battery preparation, and in particular to a back-contact battery preparation method and a back-contact battery capable of reducing the risk of gate line short circuit. Background Art
[0002] In the back-contact battery manufactured by the existing process, the electrode distribution method is a bridging method in which the main grid is perpendicular to the fine grid. Specifically, the first semiconductor main grid is vertically connected to the first semiconductor fine grid, and the second semiconductor main grid is vertically connected to the second semiconductor fine grid. The first semiconductor main grid spans over the second semiconductor fine grid and is isolated by an insulating block to avoid short circuit. Similarly, the second semiconductor main grid spans over the first semiconductor fine grid and is also isolated by an insulating block.
[0003] The prior art back contact battery preparation process has the technical problem of easily causing local short circuits, resulting in reduced battery efficiency. Summary of the invention
[0004] The present invention provides a method for preparing a back-contact battery with reduced risk of grid line short circuit and a back-contact battery, which can reduce the risk of grid line short circuit and improve battery efficiency.
[0005] The embodiments of the present invention can be implemented as follows:
[0006] An embodiment of the present invention provides a method for preparing a back-contact battery with reduced gate line short circuit risk, comprising:
[0007] Grooving the back side of the silicon wafer;
[0008] forming a first semiconductor layer and a mask layer on the back side of the silicon wafer;
[0009] forming a second semiconductor opening region on the back side of the silicon wafer;
[0010] forming a second semiconductor layer on the back side of the silicon wafer;
[0011] forming a first semiconductor opening region on the back side of the silicon wafer;
[0012] Forming metal electrodes at the positions of the first semiconductor opening area and the second semiconductor opening area on the back of the silicon wafer, respectively, printing insulating blocks on the metal electrodes, and subjecting the solidified silicon wafer to plasma defoaming treatment, wherein the insulating blocks are arranged above the grooves on the back of the silicon wafer;
[0013] The cured silicon wafer is subjected to plasma defoaming treatment.
[0014] Optionally, the step of cutting grooves on the back side of the silicon wafer includes:
[0015] Laser is used to form multiple grooves in the first semiconductor opening area and the second semiconductor opening area on the back of the silicon wafer. The length direction of the grooves is parallel to the setting direction of the fine gates, and the width direction of the grooves is parallel to the setting direction of the main gates.
[0016] Optionally, the step of cutting grooves on the back side of the silicon wafer further comprises:
[0017] The depth of the groove on the silicon wafer ranges from 30um to 45um, the width of the groove ranges from 0.5mm to 0.9mm, and the length of the groove ranges from 2mm to 6mm.
[0018] Optionally, metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back of the silicon wafer, respectively, insulating blocks are printed on the metal electrodes, and the solidified silicon wafer is subjected to plasma defoaming treatment, wherein the step of arranging the insulating block above the groove on the back of the silicon wafer includes:
[0019] First fine gate electrodes and second fine gate electrodes are alternately formed on the surfaces of the first semiconductor opening region and the second semiconductor opening region, and then insulating blocks are printed on the first fine gate electrodes and the second fine gate electrodes respectively, and baked at 150° C. for 5 min-10 min for curing.
[0020] Optionally, metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back side of the silicon wafer, respectively, insulating blocks are printed on the metal electrodes, and the solidified silicon wafer is subjected to plasma defoaming treatment, wherein the step of arranging the insulating block above the groove on the back side of the silicon wafer further includes:
[0021] The position of the insulating block corresponds to the position of the groove. The groove is provided under each insulating block. When the silver paste of the first fine gate electrode and the second fine gate electrode passes through the groove position, the silver paste is sunken into the groove. When printing the first fine gate electrode, the second fine gate electrode and the insulating block, the insulating ink is filled in the groove.
[0022] Optionally, metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back side of the silicon wafer, respectively, insulating blocks are printed on the metal electrodes, and the solidified silicon wafer is subjected to plasma defoaming treatment, wherein the step of arranging the insulating block above the groove on the back side of the silicon wafer further includes:
[0023] The first main gate electrode and the second main gate electrode are alternately printed in the vertical direction of the fine gate, the first main gate electrode and the first fine gate electrode are vertically cross-connected, the first main gate electrode and the second fine gate electrode are isolated and insulated by an insulating block, the second main gate electrode and the second fine gate electrode are vertically cross-connected, the second main gate electrode and the first fine gate electrode are isolated and insulated by the insulating block.
[0024] Optionally, metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back side of the silicon wafer, respectively, insulating blocks are printed on the metal electrodes, and the solidified silicon wafer is subjected to plasma defoaming treatment, wherein the step of arranging the insulating block above the groove on the back side of the silicon wafer further includes:
[0025] The width of the first fine gate electrode and the second fine gate electrode is 20um-40um, and the width of the first main gate electrode and the second main gate electrode is 80um-100um.
[0026] Optionally, metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back side of the silicon wafer, respectively, insulating blocks are printed on the metal electrodes, and the solidified silicon wafer is subjected to plasma defoaming treatment, wherein the step of arranging the insulating block above the groove on the back side of the silicon wafer further includes:
[0027] The solidified silicon wafer is placed in a plasma cleaning machine, a mixed gas containing hydrogen and argon is introduced into the plasma cleaning machine, the mixed gas containing hydrogen and argon is excited into plasma, and the silicon wafer is treated with plasma for 0.5min-5min at a temperature of 100℃-200℃.
[0028] Optionally, metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back side of the silicon wafer, respectively, insulating blocks are printed on the metal electrodes, and the solidified silicon wafer is subjected to plasma defoaming treatment, wherein the step of arranging the insulating block above the groove on the back side of the silicon wafer further includes:
[0029] A mixed gas containing hydrogen and argon at a flow rate of 1000sccm-10000sccm is introduced into the plasma cleaning machine, wherein the volume content of hydrogen in the mixed gas is 1%-10%, and the power density of the plasma excited by the mixed gas containing hydrogen and argon is 0.0125w / cm 2 -0.05w / cm 2 .
[0030] The present invention also provides a back-contact battery, which is prepared by a back-contact battery preparation method that reduces the risk of grid line short circuit.
[0031] The beneficial effects of the back-contact battery preparation method and the back-contact battery with reduced gate line short circuit risk according to the embodiments of the present invention include, for example:
[0032] The back contact battery preparation method for reducing the risk of gate line short circuit includes the following steps: groove carving on the back of a silicon wafer; forming a first semiconductor layer and a mask layer on the back of the silicon wafer; forming a second semiconductor opening area on the back of the silicon wafer; forming a second semiconductor layer on the back of the silicon wafer; forming a first semiconductor opening area on the back of the silicon wafer; forming metal electrodes at the positions of the first semiconductor opening area and the second semiconductor opening area on the back of the silicon wafer, printing an insulating block on the metal electrode, and performing plasma defoaming treatment on the solidified silicon wafer, wherein the insulating block is arranged above the groove on the back of the silicon wafer; performing plasma defoaming treatment on the solidified silicon wafer. During the preparation, a groove is carved on the back of the silicon wafer, and after metal electrodes are formed at the positions of the first semiconductor opening area and the second semiconductor opening area on the back of the silicon wafer, respectively, since the insulating block is arranged above the groove on the back of the silicon wafer, when printing the insulating block and printing the metal electrode, the silver paste of the printed metal electrode and the printed insulating ink can be filled in the groove, so as to avoid uneven distribution of the insulating block caused by the surface protrusion of the metal electrode, and also to avoid the printed silver paste penetrating the insulating block and connecting with the fine gate to cause a short circuit, thereby avoiding reducing the efficiency of the battery.
[0033] The back contact battery is manufactured by adopting a back contact battery manufacturing method which reduces the risk of grid line short circuit, thereby improving battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 A schematic structural diagram of a back-contact battery provided in this embodiment from a first viewing angle;
[0036] Figure 2 A schematic structural diagram of a back contact battery provided in this embodiment from a second viewing angle;
[0037] Figure 3 A schematic structural diagram of a back contact battery provided in this embodiment from a third viewing angle;
[0038] Figure 4 A schematic structural diagram of a back-contact battery provided in this embodiment from a fourth viewing angle;
[0039] Figure 5A schematic structural diagram of a back-contact battery provided in this embodiment from a fifth viewing angle;
[0040] Figure 6 A schematic structural diagram of the back-contact battery provided in this embodiment from a sixth viewing angle.
[0041] Icons: 1-silicon wafer; 1a-groove; W1-first semiconductor opening area; W2-second semiconductor opening area; W3-insulating groove; 10a-first fine gate electrode; 10b-second fine gate electrode; 11a-first main gate electrode; 11b-second main gate electrode; 12-insulating block. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0043] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0045] In the description of the present invention, it should be noted that if the terms "upper", "lower", "inside", "outside", etc. appear to indicate an orientation or position relationship, they are based on the orientation or position relationship shown in the accompanying drawings, or are the orientation or position relationship in which the product of the invention is usually placed when used. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0046] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.
[0047] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention may be combined with each other.
[0048] The electrode distribution method of the back-contact battery in the existing process is a bridging method in which the main grid is perpendicular to the fine grid. Specifically, the first semiconductor main grid is vertically connected to the first semiconductor fine grid, and the second semiconductor main grid is vertically connected to the second semiconductor fine grid. The first semiconductor main grid spans over the second semiconductor fine grid and is isolated by an insulating block to avoid short circuit. Similarly, the second semiconductor main grid spans over the first semiconductor fine grid and is also isolated by an insulating block. Since the fine grid in the prior art is raised, the insulating block ink is printed on the fine grid, which easily leads to uneven distribution of the insulating block on the fine grid. When the main grid is printed on the insulating block again and baked at high temperature, the main grid silver paste easily penetrates the insulating block and connects with the fine grid, causing local short circuit and reducing battery efficiency.
[0049] Please refer to Figure 1-Figure 6 This embodiment provides a back-contact battery preparation method and a back-contact battery that reduce the risk of gate line short circuit, which can effectively improve the above-mentioned technical problems, reduce the risk of gate line short circuit, and improve battery efficiency.
[0050] The method for preparing a back contact battery with reduced gate line short circuit risk comprises:
[0051] S1: Grooving is performed on the back side of silicon wafer 1.
[0052] Specifically, a laser is used to form multiple grooves 1a in the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back side of the silicon wafer 1. The length direction of the grooves 1a is parallel to the setting direction of the fine gate, and the width direction of the grooves 1a is parallel to the setting direction of the main gate.
[0053] In this embodiment, the depth of the groove 1a on the silicon wafer 1 is in the range of 30um-45um, the width of the groove 1a is in the range of 0.5mm-0.9mm, and the length of the groove 1a is in the range of 2mm-6mm.
[0054] S2: Polishing the front and back sides of the silicon wafer 1.
[0055] Specifically, the front and back sides of the silicon wafer 1 are polished and cleaned, and the polishing solution is a mixture of potassium hydroxide or sodium hydroxide and water, wherein the mass percentage of sodium hydroxide or potassium hydroxide is 10%-20%, and the polishing time is 5min-15min.
[0056] S3: forming a first semiconductor layer and a mask layer on the back side of the silicon wafer 1 .
[0057] Specifically, the first semiconductor layer includes a tunneling silicon oxide layer and an N-type doped polysilicon layer, wherein the tunneling silicon oxide layer has a thickness of 1 nm-2 nm, and the N-type doped polysilicon layer has a thickness of 70 nm-120 nm.
[0058] The mask layer is at least one of silicon nitride, silicon oxide, silicon oxynitride or nitrogen-containing polysilicon, preferably silicon nitride, and the thickness of the mask layer is 40nm-90nm.
[0059] In this embodiment, the tunneling silicon oxide layer, the N-type doped polysilicon layer and the mask layer are sequentially deposited and annealed at high temperature using a tubular polysilicon deposition furnace, and the deposition temperature is 400°C-500°C; when depositing the tunneling oxide layer, the mass flow rate of laughing gas is 8000sccm-1200sccm, the pressure is 100pa-200pa, the power supply power is 3KW-20KW, and the deposition time is 20s-100s; when depositing the N-type doped polysilicon layer, the mass flow rate of silane is 1000sccm-3000sccm, the mass flow rate of phosphine (2% PH3 / 98% H2) is 1000sccm-2500sccm, the mass flow rate of hydrogen is 7000sccm-9000sccm, the pressure is 400pa-500pa, the power supply power is 5KW-20KW, and the time is 800s-1300s; when depositing the mask layer, the mass flow rate of silane is 1000 sccm -2000sccm, the mass flow rate of nitrogen is 2000sccm -5000sccm, the pressure is 200pa-300pa, the power is 3KW -20KW, and the time is 300s-800s; nitrogen needs to be introduced during high-temperature annealing, the mass flow rate of nitrogen is 5000sccm -15000sccm, the annealing temperature is 850℃-950℃, the pressure is 1000pa-10000pa, and the time is 40min-60min.
[0060] S4: forming a second semiconductor opening region W2 on the back side of the silicon wafer 1 .
[0061] Specifically, a first opening is etched on the back of the silicon wafer 1 by laser or mask etching to form a second semiconductor opening area W2, wherein the laser can be a green laser or an ultraviolet laser, the laser pulse width is less than 10ns, and the width of the formed second semiconductor opening area W2 is 400um-600um.
[0062] S5: Perform texturing and cleaning on the opening areas on the front and back sides of the silicon wafer 1.
[0063] Specifically, a mixture of potassium hydroxide or sodium hydroxide, a texturing additive and water is used to texturing and clean the opening areas on the front and back sides of the silicon wafer 1, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1%-5%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 8min-30min, and the texturing temperature is 75℃-85℃.
[0064] In this embodiment, during the front texturing process, the silicon nitride mask layer on the back of the silicon wafer 1 is also removed simultaneously through the final cleaning solution. The solution used to remove the mask layer is an acid solution such as HF, the mass percentage of HF acid is 0.5%-5%, the mass percentage of deionized water is 95%-99.5%, the processing temperature is 20℃-30℃, and the removal time is 60s-300s.
[0065] S6: forming a second semiconductor layer on the back side of the silicon wafer 1 .
[0066] Specifically, the second semiconductor layer may be a stack of an intrinsic hydrogenated amorphous silicon layer and a P-type doped amorphous / microcrystalline silicon layer, or may be a stack of a tunneling silicon oxide layer and a P-type doped polycrystalline silicon layer.
[0067] When the second semiconductor layer is a stack of an intrinsic hydrogenated amorphous silicon layer and a P-type doped amorphous / microcrystalline silicon layer, the second semiconductor layer is formed by a plate CVD method, wherein the thickness of the intrinsic hydrogenated amorphous silicon layer is 4nm-8nm, the thickness of the stack of P-type doped amorphous / microcrystalline silicon layers is 6nm-12nm, and the deposition temperature of the second semiconductor layer is 150℃-250℃.
[0068] S7: forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer 1.
[0069] Specifically, the passivation layer can be one or a combination of an amorphous silicon passivation layer, a silicon oxide passivation layer and an aluminum oxide passivation layer, preferably a combination of silicon oxide and aluminum oxide passivation layers, the thickness of silicon oxide is 1nm-2nm, and the thickness of aluminum oxide is 3nm-4nm.
[0070] The anti-reflection layer can be one or a combination of silicon nitride, aluminum oxide and silicon oxide layers, preferably a combination of silicon nitride and silicon oxide. The thickness of silicon nitride is 50nm-100nm, and the thickness of silicon oxide is 30nm-120nm.
[0071] S8: forming a first semiconductor opening region W1 on the back side of the silicon wafer 1 .
[0072] Specifically, a second etching opening is performed on the back side of the silicon wafer 1 by laser to form a first semiconductor opening area W1. The laser can be a green laser or an ultraviolet laser. The laser pulse width is less than 10ns. The width of the formed first semiconductor opening area W1 is 100um-250um.
[0073] S9: depositing a conductive film layer on the back side of the silicon wafer 1 .
[0074] Specifically, a transparent conductive film is deposited on the back of the silicon wafer 1 by physical vapor deposition technology or activated plasma deposition technology. The thickness of the transparent conductive film is 40nm-80nm. The material of the transparent conductive film can be an indium oxide-based film doped with tin, tungsten, titanium, or zinc, or an aluminum / boron-doped zinc oxide-based film.
[0075] S10: performing a third etching opening on the back side of the silicon wafer 1 to form an insulating groove W3.
[0076] Specifically, an opening is etched on the back side of the silicon wafer 1 by mask etching or laser to form an insulating groove W3 between the first semiconductor and the second semiconductor. The width of the insulating groove W3 is 20 μm-100 μm. After etching, the resistance between the first semiconductor and the second semiconductor is greater than 1 KΩ.
[0077] S11: Metal electrodes are formed at the positions of the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back side of the silicon wafer 1, respectively, an insulating block 12 is printed on the metal electrodes, and the solidified silicon wafer 1 is subjected to plasma defoaming treatment, wherein the insulating block 12 is arranged above the groove 1a on the back side of the silicon wafer 1.
[0078] Specifically, the metal electrode includes a fine gate electrode and a main gate electrode, and the metal electrodes are formed at the positions of the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back side of the silicon wafer 1 by screen printing technology; wherein, the first fine gate electrode 10a and the second fine gate electrode 10b are first formed alternately on the surface of the first semiconductor opening area W1 and the second semiconductor opening area W2, and then the insulating block 12 is printed on the first fine gate electrode 10a and the second fine gate electrode 10b respectively, and baked at a temperature of 150°C for 5min-10min for curing.
[0079] The thickness of the insulating block 12 is 5um-20um, the length of the insulating block 12 is 3mm-5mm, the width of the insulating block 12 is 0.5mm-1mm, the position of the insulating block 12 corresponds to the position of the groove 1a, and a groove 1a is provided under each insulating block 12. When the silver paste of the first fine gate electrode 10a and the second fine gate electrode 10b passes through the position of the groove 1a, the silver paste is sunken in the groove 1a. When printing the first fine gate electrode 10a, the second fine gate electrode 10b and the insulating block 12, the insulating ink is filled in the groove 1a.
[0080] Then, the solidified silicon wafer 1 is placed in a plasma cleaning machine for plasma defoaming treatment, and a mixed gas containing hydrogen and argon is introduced into the plasma cleaning machine to excite the mixed gas containing hydrogen and argon into plasma, and the silicon wafer 1 is treated with plasma for 0.5min-5min at a temperature of 100°C-200°C. Specifically, a mixed gas containing hydrogen and argon with a flow rate of 1000sccm-10000sccm is introduced into the plasma cleaning machine, wherein the volume content of hydrogen in the mixed gas is 1%-10%, and the power density of the plasma excited by the mixed gas containing hydrogen and argon is 0.0125w / cm 2 -0.05w / cm 2 , which can be beneficial to controlling the defoaming effect and the purging effect. It can not only allow the plasma treatment to eliminate the bubbles formed during the curing of the insulating ink, make up for the defects and improve the isolation effect of the insulating ink, but also allow the plasma treatment to remove the loose particle impurities on the surface of the silicon wafer 1 and the surface of the fine grid, further improve the bonding force between the main grid and the fine grid, and improve the electrode connection effect.
[0081] The back side of the silicon wafer 1 is grooved by using an ultraviolet laser or a green laser with a pulse width less than 10 ns.
[0082] After the silicon wafer 1 is subjected to plasma defoaming treatment, a first main gate electrode 11a and a second main gate electrode 11b are alternately printed in a vertical direction of the fine gates, the first main gate electrode 11a and the first fine gate electrode 10a are vertically cross-connected, the first main gate electrode 11a and the second fine gate electrode 10b are isolated and insulated by an insulating block 12, the second main gate electrode 11b and the second fine gate electrode 10b are vertically cross-connected, the second main gate electrode 11b and the first fine gate electrode 10a are isolated and insulated by the insulating block 12, the first main gate electrode 11a, the insulating block 12 and the second fine gate electrode 10b are vertically cross-connected, The intersection of the electrode 10b is located at the position of the groove 1a, and the intersection of the second main gate electrode 11b, the insulating block 12 and the first fine gate electrode 10a is also located at the position of the groove 1a. When the silver paste of the first fine gate electrode 10a and the silver paste of the second fine gate electrode 10b pass through the groove 1a, they are embedded in the groove 1a, and the insulating ink is filled on the groove 1a. The insulating block 12 will not have different thicknesses due to the protrusion of the fine gate, and the silver paste of the first main gate electrode 11a and the silver paste of the second main gate electrode 11b are not easy to penetrate the insulating block 12 and the fine gate to cause a short circuit, thereby forming a good insulation effect.
[0083] The width of the first fine gate electrode 10a and the second fine gate electrode 10b is 20um-40um, the width of the first main gate electrode 11a and the second main gate electrode 11b is 80um-100um, and the insulation resistance is greater than 1KΩ.
[0084] In summary, an embodiment of the present invention provides a back-contact battery preparation method and a back-contact battery that reduce the risk of gate line short circuit. The back-contact battery preparation method that reduces the risk of gate line short circuit includes grooves on the back side of the silicon wafer 1; forming a first semiconductor layer and a mask layer on the back side of the silicon wafer 1; forming a second semiconductor opening area W2 on the back side of the silicon wafer 1; forming a second semiconductor layer on the back side of the silicon wafer 1; forming a first semiconductor opening area W1 on the back side of the silicon wafer 1; forming metal electrodes at the positions of the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back side of the silicon wafer 1, respectively, printing an insulating block 12 on the metal electrode, and performing plasma defoaming treatment on the cured silicon wafer 1, wherein the insulating block 12 is arranged above the groove 1a on the back side of the silicon wafer 1; and performing plasma defoaming treatment on the cured silicon wafer 1. During the preparation, a groove 1a is engraved on the back of the silicon wafer 1. After metal electrodes are formed at the positions of the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back of the silicon wafer 1, since the insulating block 12 is arranged above the groove 1a on the back of the silicon wafer 1, when printing the insulating block 12 and printing the metal electrode, the silver paste of the printed metal electrode and the printed insulating ink can be filled in the groove 1a, avoiding the uneven distribution of the insulating block 12 caused by the surface protrusion of the metal electrode, and avoiding the printed silver paste from penetrating the insulating block 12 and connecting with the fine grid to cause a short circuit, thereby avoiding reducing the efficiency of the battery.
[0085] The back contact battery is manufactured by adopting a back contact battery manufacturing method which reduces the risk of grid line short circuit, thereby improving battery efficiency.
[0086] Example 1
[0087] A method for preparing a back contact battery with reduced gate line short circuit risk includes:
[0088] S1: Grooving is performed on the back side of silicon wafer 1.
[0089] The depth of the groove 1a on the silicon wafer 1 is 38 um, the width of the groove 1a is 0.7 mm, and the length of the groove 1a is 4 mm.
[0090] S2: Polishing the front and back sides of the silicon wafer 1.
[0091] S3: forming a first semiconductor layer and a mask layer on the back side of the silicon wafer 1 .
[0092] The first semiconductor layer includes a tunneling silicon oxide layer and an N-type doped polysilicon layer, wherein the tunneling silicon oxide layer has a thickness of 1.5 nm and the N-type doped polysilicon layer has a thickness of 120 nm.
[0093] The mask layer is at least one of silicon nitride, silicon oxide, silicon oxynitride or nitrogen-containing polysilicon, preferably silicon nitride, and the thickness of the mask layer is 70 nm.
[0094] S4: forming a second semiconductor opening region W2 on the back side of the silicon wafer 1 .
[0095] The first opening is etched on the back of the silicon wafer 1 by laser or mask etching to form a second semiconductor opening area W2, wherein the laser can be a green laser or an ultraviolet laser, the laser pulse width is less than 10ns, and the width of the formed second semiconductor opening area W2 is 500um.
[0096] S5: Perform texturing and cleaning on the opening areas on the front and back sides of the silicon wafer 1.
[0097] S6: forming a second semiconductor layer on the back side of the silicon wafer 1 .
[0098] The second semiconductor layer may be a stack of an intrinsic hydrogenated amorphous silicon layer and a P-type doped amorphous / microcrystalline silicon layer, or may be a stack of a tunneling silicon oxide layer and a P-type doped polycrystalline silicon layer.
[0099] When the second semiconductor layer is a stack of an intrinsic hydrogenated amorphous silicon layer and a P-type doped amorphous / microcrystalline silicon layer, the second semiconductor layer is formed by a plate-type CVD method, wherein the thickness of the intrinsic hydrogenated amorphous silicon layer is 8nm, the thickness of the stack of P-type doped amorphous / microcrystalline silicon layers is 13nm, and the deposition temperature of the second semiconductor layer is 150°C-250°C.
[0100] S7: forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer 1.
[0101] The passivation layer can be one or a combination of an amorphous silicon passivation layer, a silicon oxide passivation layer and an aluminum oxide passivation layer, preferably a combination of silicon oxide and aluminum oxide passivation layers, the thickness of silicon oxide is 0.85 nm, and the thickness of aluminum oxide is 3.5 nm.
[0102] The anti-reflection layer can be one or a combination of silicon nitride, aluminum oxide and silicon oxide layers, preferably a combination of silicon nitride and silicon oxide, the thickness of silicon nitride is 75 nm, and the thickness of silicon oxide is 100 nm.
[0103] S8: forming a first semiconductor opening region W1 on the back side of the silicon wafer 1 .
[0104] A second etching opening is performed on the back side of the silicon wafer 1 by laser to form a first semiconductor opening area W1. The laser can be a green laser or an ultraviolet laser. The laser pulse width is less than 10ns. The width of the formed first semiconductor opening area W1 is 230um.
[0105] S9: depositing a conductive film layer on the back side of the silicon wafer 1 .
[0106] A transparent conductive film is deposited on the back of the silicon wafer 1 by physical vapor deposition technology or activated plasma deposition technology. The thickness of the transparent conductive film is 70nm. The material of the transparent conductive film can be an indium oxide-based film doped with tin, tungsten, titanium, or zinc, or an aluminum / boron-doped zinc oxide-based film.
[0107] S10: performing a third etching opening on the back side of the silicon wafer 1 to form an insulating groove W3.
[0108] Specifically, an opening is etched on the back side of the silicon wafer 1 by mask etching or laser to form an insulating groove W3 between the first semiconductor and the second semiconductor. The width of the insulating groove W3 is 90 μm. After etching, the resistance between the first semiconductor and the second semiconductor is greater than 1 KΩ.
[0109] S11: Metal electrodes are formed at the positions of the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back side of the silicon wafer 1, respectively, an insulating block 12 is printed on the metal electrodes, and the solidified silicon wafer 1 is subjected to plasma defoaming treatment, wherein the insulating block 12 is arranged above the groove 1a on the back side of the silicon wafer 1.
[0110] Specifically, the metal electrode includes a fine gate electrode and a main gate electrode, and the metal electrodes are formed at the positions of the first semiconductor opening area W1 and the second semiconductor opening area W2 on the back side of the silicon wafer 1 by screen printing technology; wherein, the first fine gate electrode 10a and the second fine gate electrode 10b are first formed alternately on the surface of the first semiconductor opening area W1 and the second semiconductor opening area W2, and then the insulating block 12 is printed on the first fine gate electrode 10a and the second fine gate electrode 10b respectively, and baked at a temperature of 150°C for 5min-10min for curing.
[0111] The thickness of the insulating block 12 is 15um, the length of the insulating block 12 is 4mm, and the width of the insulating block 12 is 0.75mm. The position of the insulating block 12 corresponds to the position of the groove 1a one by one. A groove 1a is provided under each insulating block 12. When the silver paste of the first fine gate electrode 10a and the second fine gate electrode 10b passes through the position of the groove 1a, the silver paste is sunken in the groove 1a. When printing the first fine gate electrode 10a, the second fine gate electrode 10b and the insulating block 12, the insulating ink is filled in the groove 1a.
[0112] Then, the solidified silicon wafer 1 is placed in a plasma cleaning machine for plasma defoaming treatment, and a mixed gas containing hydrogen and argon is introduced into the plasma cleaning machine to excite the mixed gas containing hydrogen and argon into plasma, and the silicon wafer 1 is treated with plasma for 3.5 minutes at a temperature of 180°C. Specifically, a mixed gas containing hydrogen and argon with a flow rate of 4500sccm is introduced into the plasma cleaning machine, wherein the volume content of hydrogen in the mixed gas is 6%, and the power density of the plasma excited by the mixed gas containing hydrogen and argon is 0.025w / cm 2 , which can be beneficial to controlling the defoaming effect and the purging effect. It can not only allow the plasma treatment to eliminate the bubbles formed during the curing of the insulating ink, make up for the defects and improve the isolation effect of the insulating ink, but also allow the plasma treatment to remove the loose particle impurities on the surface of the silicon wafer 1 and the surface of the fine grid, further improve the bonding force between the main grid and the fine grid, and improve the electrode connection effect.
[0113] The back side of the silicon wafer 1 is grooved by using an ultraviolet laser or a green laser with a pulse width less than 10 ns.
[0114] After the silicon wafer 1 is subjected to plasma defoaming treatment, a first main gate electrode 11a and a second main gate electrode 11b are alternately printed in a vertical direction of the fine gates, the first main gate electrode 11a and the first fine gate electrode 10a are vertically cross-connected, the first main gate electrode 11a and the second fine gate electrode 10b are isolated and insulated by an insulating block 12, the second main gate electrode 11b and the second fine gate electrode 10b are vertically cross-connected, the second main gate electrode 11b and the first fine gate electrode 10a are isolated and insulated by the insulating block 12, the first main gate electrode 11a, the insulating block 12 and the second fine gate electrode 10b are vertically cross-connected, The intersection of the electrode 10b is located at the position of the groove 1a, and the intersection of the second main gate electrode 11b, the insulating block 12 and the first fine gate electrode 10a is also located at the position of the groove 1a. When the silver paste of the first fine gate electrode 10a and the silver paste of the second fine gate electrode 10b pass through the groove 1a, they are embedded in the groove 1a, and the insulating ink is filled on the groove 1a. The insulating block 12 will not have different thicknesses due to the protrusion of the fine gate, and the silver paste of the first main gate electrode 11a and the silver paste of the second main gate electrode 11b are not easy to penetrate the insulating block 12 and the fine gate to cause a short circuit, thereby forming a good insulation effect.
[0115] The width of the first fine gate electrode 10a and the second fine gate electrode 10b is 30 um, and the width of the first main gate electrode 11a and the second main gate electrode 11b is 85 um. The insulation resistance is greater than 1 KΩ.
[0116] Example 2
[0117] The process is carried out with reference to Example 1, except that the width of the groove 1a is 0.5 mm.
[0118] Example 3
[0119] The process is carried out with reference to Example 1, except that the depth of the groove 1a is 30 um.
[0120] Example 4
[0121] The process is carried out with reference to Example 1, except that the length of the groove 1a is 2.5 mm.
[0122] Example 5
[0123] The process is carried out with reference to Example 1, except that the plasma treatment is carried out at a temperature of 120° C. for the silicon wafer 1 .
[0124] Example 6
[0125] The process is carried out with reference to Example 1, except that the silicon wafer 1 is treated with plasma for 0.8 min.
[0126] Example 7
[0127] The process is carried out with reference to Example 1, except that a mixed gas containing hydrogen and argon with a flow rate of 1000 sccm is introduced into the plasma cleaning machine.
[0128] Example 8
[0129] The process is carried out with reference to Example 1, except that the volume content of hydrogen in the mixed gas is 1%.
[0130] Example 9
[0131] The method is carried out in accordance with Example 1. The difference from Example 1 is that the power density of the plasma excited by the mixed gas containing hydrogen and argon is 0.013w / cm 2 .
[0132] Comparative Example 1
[0133] The process is carried out with reference to Example 1, except that the width of the groove 1a is 0.3 mm.
[0134] Comparative Example 2
[0135] The process is carried out with reference to Example 1, except that the depth of the groove 1a is 15 um.
[0136] Comparative Example 3
[0137] The process is carried out with reference to Example 1, except that the length of the groove 1a is 1 mm.
[0138] Comparative Example 4
[0139] The process is carried out with reference to Example 1, except that the plasma treatment is carried out at a temperature of 250° C. for the silicon wafer 1 .
[0140] Comparative Example 5
[0141] The process is carried out with reference to Example 1, except that the silicon wafer 1 is treated with plasma for 15 minutes.
[0142] Comparative Example 6
[0143] The process is carried out with reference to Example 1, except that a mixed gas containing hydrogen and argon with a flow rate of 200 sccm is introduced into the plasma cleaning machine.
[0144] Comparative Example 7
[0145] The process is carried out with reference to Example 1, except that the volume content of hydrogen in the mixed gas is 0.15%.
[0146] Comparative Example 8
[0147] The method is carried out in accordance with Example 1. The difference from Example 1 is that the power density of the plasma excited by the mixed gas containing hydrogen and argon is 0.1w / cm 2 .
[0148] Comparative Example 9
[0149] The process is carried out with reference to Example 1, except that no groove 1 a is provided on the back side of the silicon wafer 1 .
[0150] Comparative Example 10
[0151] The process is carried out with reference to Example 1, but different from Example 1, the silicon wafer 1 after curing is not subjected to plasma defoaming treatment.
[0152] Comparative Example 11
[0153] The process is carried out with reference to Example 1. The difference from Example 1 is that no groove 1a is provided on the back of the silicon wafer 1, and the silicon wafer 1 after curing is not subjected to plasma defoaming treatment.
[0154] Test Case
[0155] The open circuit voltage, parallel resistance, fill factor and conversion efficiency of the back contact cells obtained in the above embodiments and comparative examples were respectively tested for performance, and the results are shown in Table 1, wherein the test method is to perform performance tests on the manufactured cells on an IV tester.
[0156] Table 1
[0157]
[0158] It can be seen from the above results that, compared with the comparative example, the embodiment scheme of the present invention, which adopts the method of groove engraving under the back insulating block combined with plasma to eliminate bubbles, can effectively reduce the risk of short circuit, which is beneficial to the improvement of parallel resistance and fill factor. Furthermore, according to Examples 1 and Examples 2-9, it can be seen that the preferred parameter scheme of the present invention can better take into account the passivation and insulation effects, which is beneficial to the improvement of battery conversion efficiency.
[0159] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a back contact battery with reduced gate line short circuit risk, It is characterized in that include: Grooving is performed on the back of a silicon wafer (1); wherein a plurality of grooves (1a) are formed in a first semiconductor opening region (W1) and a second semiconductor opening region (W2) on the back of the silicon wafer (1) using a laser, wherein the length direction of the grooves (1a) is parallel to the setting direction of the fine gate, and the width direction of the grooves (1a) is parallel to the setting direction of the main gate; Forming a first semiconductor layer and a mask layer on the back side of the silicon wafer (1); forming a second semiconductor opening region (W2) on the back side of the silicon wafer (1); forming a second semiconductor layer on the back side of the silicon wafer (1); Forming a first semiconductor opening region (W1) on the back side of the silicon wafer (1); Forming metal electrodes at the positions of the first semiconductor opening region (W1) and the second semiconductor opening region (W2) on the back side of the silicon wafer (1), printing insulating blocks (12) on the metal electrodes, and subjecting the solidified silicon wafer (1) to a plasma defoaming treatment, wherein the insulating blocks (12) are arranged above the groove (1a) on the back side of the silicon wafer (1); alternately forming first fine gate electrodes (10a) and second fine gate electrodes (10b) on the surfaces of the first semiconductor opening region (W1) and the second semiconductor opening region (W2), then printing insulating blocks (12) on the first fine gate electrodes (10a) and the second fine gate electrodes (10b), and baking at a temperature of 150°C for 5 min-10 min for solidification; The position of the insulating block (12) corresponds to the position of the groove (1a) one by one, and the groove (1a) is provided below each insulating block (12); when the silver paste of the first fine gate electrode (10a) and the second fine gate electrode (10b) pass through the position of the groove (1a), the silver paste is sunken into the groove (1a); when the first fine gate electrode (10a), the second fine gate electrode (10b) and the insulating block (12) are printed, the insulating ink is filled into the groove (1a).
2. The method for preparing a back-contact battery with reduced gate line short circuit risk according to claim 1, It is characterized in that The step of engraving grooves on the back side of the silicon wafer (1) further comprises: The depth of the groove (1a) on the silicon wafer (1) ranges from 30um to 45um, the width of the groove (1a) ranges from 0.5mm to 0.9mm, and the length of the groove (1a) ranges from 2mm to 6mm.
3. The method for preparing a back-contact battery with reduced gate line short circuit risk according to claim 1, It is characterized in that The steps of forming metal electrodes at the positions of the first semiconductor opening region (W1) and the second semiconductor opening region (W2) on the back side of the silicon wafer (1), printing insulating blocks (12) on the metal electrodes, and subjecting the solidified silicon wafer (1) to plasma defoaming treatment, wherein the step of arranging the insulating block (12) above the groove (1a) on the back side of the silicon wafer (1) further comprises: A first main gate electrode (11a) and a second main gate electrode (11b) are alternately printed in a vertical direction of the fine gate, the first main gate electrode (11a) and the first fine gate electrode (10a) are vertically cross-connected, the first main gate electrode (11a) and the second fine gate electrode (10b) are isolated and insulated by an insulating block (12), the second main gate electrode (11b) and the second fine gate electrode (10b) are vertically cross-connected, and the second main gate electrode (11b) and the first fine gate electrode (10a) are isolated and insulated by the insulating block (12).
4. The method for preparing a back-contact battery with reduced gate line short circuit risk according to claim 3, It is characterized in that The steps of forming metal electrodes at the positions of the first semiconductor opening region (W1) and the second semiconductor opening region (W2) on the back side of the silicon wafer (1), printing insulating blocks (12) on the metal electrodes, and subjecting the solidified silicon wafer (1) to plasma defoaming treatment, wherein the step of arranging the insulating block (12) above the groove (1a) on the back side of the silicon wafer (1) further comprises: The width of the formed first fine gate electrode (10a) and the second fine gate electrode (10b) is 20um-40um, and the width of the formed first main gate electrode (11a) and the second main gate electrode (11b) is 80um-100um.
5. The method for preparing a back contact battery with reduced gate line short circuit risk according to claim 1, It is characterized in that The steps of forming metal electrodes at the positions of the first semiconductor opening region (W1) and the second semiconductor opening region (W2) on the back side of the silicon wafer (1), printing insulating blocks (12) on the metal electrodes, and subjecting the solidified silicon wafer (1) to plasma defoaming treatment, wherein the step of arranging the insulating block (12) above the groove (1a) on the back side of the silicon wafer (1) further comprises: The solidified silicon wafer (1) is placed in a plasma cleaning machine, a mixed gas containing hydrogen and argon is introduced into the plasma cleaning machine, the mixed gas containing hydrogen and argon is excited into plasma, and the silicon wafer (1) is treated with plasma for 0.5 min to 5 min at a temperature of 100° C. to 200° C.
6. The method for preparing a back contact battery with reduced gate line short circuit risk according to claim 4, It is characterized in that The steps of forming metal electrodes at the positions of the first semiconductor opening region (W1) and the second semiconductor opening region (W2) on the back side of the silicon wafer (1), printing insulating blocks (12) on the metal electrodes, and subjecting the solidified silicon wafer (1) to plasma defoaming treatment, wherein the step of arranging the insulating block (12) above the groove (1a) on the back side of the silicon wafer (1) further comprises: A mixed gas containing hydrogen and argon at a flow rate of 1000sccm-10000sccm is introduced into the plasma cleaning machine, wherein the volume content of hydrogen in the mixed gas is 1%-10%, and the power density of the plasma excited by the mixed gas containing hydrogen and argon is 0.0125w / cm 2 -0.05w / cm 2 .
7. A back contact battery, It is characterized in that The back contact battery is prepared by the method for preparing a back contact battery with reduced gate line short circuit risk as described in any one of claims 1 to 6.