Method for preparing solid-state energy storage battery using electroplating sludge and humic acid
The solid energy storage battery with excellent performance was prepared by hydrothermal synthesis and solution-assisted solid-phase reaction method, which solved the problem of insufficient rate performance of graphite carbonaceous materials in lithium-ion batteries, and realized electroplating sludge and humic acid Resource utilization to achieve efficient energy storage effect.
Patent Information
- Application Number
- CN202410843872.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Commercial graphite carbonaceous materials are difficult to achieve the rate performance of high current charging and discharge in lithium-ion batteries, and the resource utilization of electroplating sludge and humic acid has not been effectively solved.
Na0.6Ni0.8Co0.6O2 positive electrode material and Sn-HA/C negative electrode material were prepared by hydrothermal synthesis method, and Na3Zr2Si2PO12-HA/C electrolyte material was prepared by solution-assisted solid phase reaction method, and tableting was prepared with conductive adhesive. Solid state energy storage battery.
The resource utilization of electroplating sludge and humic acid was realized, and a solid-state energy storage battery with excellent performance was prepared, with good conductivity and energy storage performance, and a capacity retention rate of 93%.
Smart Images

Figure CN118659039B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy storage battery preparation, and in particular to a method for preparing a solid energy storage electrolyte by using electroplating sludge and humic acid. Background Art
[0002] Commercial negative electrode materials are mainly graphite-like carbon materials, but the anisotropic structural characteristics of graphite limit the free diffusion of sodium ions in the graphite structure. This property affects the rate performance of negative electrode materials prepared from graphite. Therefore, graphite-like carbon materials are difficult to be directly used as negative electrode materials in lithium-ion batteries with large current charge and discharge.
[0003] Electroplating sludge usually contains transition metals such as Fe, Cr, Sn, Ni, and Co. Nickel oxides, hydroxides, and nickel-based layered double hydroxide materials (LDH) show great application potential in supercapacitors.
[0004] Humic acid molecules contain more quinone hydroxyl groups, while fulvic acid contains more phenolic hydroxyl groups. Humic acid from the same source has a better ability to accept electrons. The quinone group in humus determines the ability to accept electrons, and the phenol group determines the ability to donate electrons. Soil humus has a strong ability to donate electrons. High-temperature carbonization of humic acid can form a multi-layer graphitized structure, and carbon materials such as graphite are commonly used negative electrodes for batteries. Therefore, how to make resource-based use of electroplating sludge and humic acid to prepare energy storage batteries is a technical problem that needs to be solved urgently. Summary of the invention
[0005] In order to realize resource utilization of electroplating sludge and humic acid, the present invention provides a method for preparing a solid-state energy storage battery by using electroplating sludge and humic acid.
[0006] The method for preparing a solid-state energy storage battery from electroplating sludge and humic acid provided by the present invention has the following main technical routes:
[0007] Na was prepared by treating nickel-rich electroplating sludge. 0.6 Ni 0.8 Co 0.6 O2 positive electrode material; Sn-HA / C negative electrode was prepared by hydrothermal synthesis; and electrolyte precursor was prepared by solution-assisted solid phase reaction method, and humic acid was doped into electrolyte precursor by doping and co-sintering to prepare humic acid-doped Na3Zr2Si2PO 12 -HA / C electrolyte material. Finally, the negative electrode material, electrolyte material and positive electrode material containing a conductive adhesive are pressed into sheets in turn, and then combined with corresponding accessories to assemble into a solid-state energy storage battery or capacitor.
[0008] The specific steps are as follows:
[0009] S1. Preparation of Na by hydrothermal synthesis using electroplating sludge as raw material 0.6 Ni 0.8 Co 0.6 O2 positive electrode material. The specific preparation steps are as follows:
[0010] S11, pretreatment of electroplating sludge: adding the dried sludge into deionized water and soaking for 8-12 minutes, then adding hydrochloric acid and stirring to obtain a uniform solution; adjusting the pH of the solution to neutral, then adding urea and stirring to dissolve, sealing the solution in a hydrothermal synthesis reactor, reacting at 110-130° C. for 12 hours, centrifuging the obtained mixture, and drying the filter residue to obtain a solid powder;
[0011] S12, dissolving NaHCO3 and CoCl4 and the solid powder obtained in step S11 in deionized water, adding sodium oxalate as a precipitant, and then transferring the obtained mixed solution to a hydrothermal synthesis reactor, and reacting at a constant temperature of 110-130°C for 12-14h, evaporating and removing the solvent after the reaction to obtain a precursor, and calcining the precursor at 500°C for 2-3h under N2 atmosphere to obtain the product Na 0.6 Ni 0.8 Co 0.6 O2 is the positive electrode material.
[0012] S2. Prepare Sn-HA / C negative electrode material by hydrothermal synthesis using humic acid and SnO2 as raw materials. The specific preparation steps are as follows:
[0013] S21, dissolving humic acid in NaOH solution, adding SnO2 to the solution, stirring evenly, then transferring the mixed solution to a hydrothermal synthesis reactor, moving the reactor to a vacuum drying oven and reacting at 120° C. for 12 h, and evaporating and removing the solvent after the reaction to obtain a solid powder;
[0014] S22. The solid powder was activated by calcining at 500°C for 2 h in a N2 atmosphere. After activation, it was rinsed with deionized water until neutral and dried. The obtained material was named Sn-HA / C and used as the negative electrode material of the battery.
[0015] S3. Preparation of Na3Zr2Si2PO4 by solution-assisted solid phase reaction method 12 -HA / C solid electrolyte material; the method is as follows:
[0016] S31, adding NaNO3 and ZrOCl2·8H2O to deionized water, adding nitric acid to make the solution pH = 1, and then adding (NH4)2HPO4 to the solution under stirring conditions, the whole solution becomes a mixture of colloidal sol and a precipitate of a complex zirconium oxyphosphate compound; shaking the mixture on a shaker for 12 hours to allow the mixture to react fully;
[0017] S32, drying the mixture obtained in step S31 to obtain a solid powder, and calcining the solid powder at 500° C. for 2 h under a N2 atmosphere to obtain an electrolyte precursor powder;
[0018] S33, SiO2 and humic acid were added to the electrolyte precursor powder, and the mixture was fully ground and calcined at 500°C for 2h in a N2 atmosphere to obtain the product Na3Zr2Si2PO 12 / HA-C solid electrolyte material.
[0019] S4. In Na 0.6 Ni 0.8 Co 0.6 O2 positive electrode material, Sn-HA / C negative electrode material and Na3Zr2Si2PO 12 -Conductive adhesives are added to the HA / C solid electrolyte materials respectively.
[0020] S5. The negative electrode material, electrolyte material and positive electrode material containing a conductive adhesive are pressed into sheets in sequence, and then assembled into a solid-state energy storage battery or capacitor in combination with corresponding accessories.
[0021] Preferably, in step S21, the mass ratio of humic acid to SnO2 is 5:2.
[0022] Preferably, in step S21, the method of dissolving humic acid in NaOH solution is: adding humic acid to a concentration of 0.5 mol·L -1 The NaOH solution was heated to 60°C and stirred at a constant temperature until the humic acid was completely dissolved in the NaOH solution.
[0023] The conductive adhesive is preferably poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), and the added amount accounts for 0.3-5% of the mass of the electrode material or the electrolyte material.
[0024] Preferably, in step S5, the preparation method of the tablet is: first pour the negative electrode powder into the mold so that the powder is evenly spread on the surface, and the tablet is pressed at a pressure of 4Mp for 20s; then continue to fill the solid electrolyte powder into the mold, and press the tablet at a pressure of 4Mp for 20s; then continue to fill the positive electrode powder, and press the tablet at a pressure of 5Mp for 20s.
[0025] Compared with the prior art, the present invention is beneficial in that:
[0026] (1) In the method of the present invention, Sn / C negative electrode material is prepared by combining humus as a carbon source with SnO2 particles; ordered mesoporous carbon is synthesized by using humic acid as a carbon source. The obtained carbonaceous material has hexagonal ordered pores, which originate from the porous structure of humic acid-derived carbon. The conductive groups formed by calcining humic acid and the voids form a carbon frame and are beneficial to conductivity and energy storage.
[0027] (2) The main components of electroplating sludge are zirconium, nickel, iron, chlorine, and phosphorus. The oxidized transition metals in the sludge are converted into metal chlorides and sulfides, such as Na3Zr2Si2PO 12 .
[0028] (3) The present invention not only realizes the resource utilization of humic acid from electroplating sludge and kitchen waste compost, but also prepares a solid-state energy storage battery with excellent performance.
[0029] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Scanning electron microscope images of Sn-HA / C powder sintered at 500°C, where (a), (b), (c) and (d) are scanning electron microscope images of the sample at different magnifications.
[0031] Figure 2 Na sintered at 500℃ 0.6 Ni 0.8 Co 0.6 Scanning electron microscope images of O2 positive electrode powder, where (a), (b), (c) and (d) are electron microscope images of the sample at different magnifications.
[0032] Figure 3 Sintered Na3Zr2Si2PO 12 -SEM images of HA / C electrolyte powder. (a), (b), (c) and (d) are SEM images of the sample at different magnifications.
[0033] Figure 4 Sintered Na3Zr2Si2PO 12 - TEM images of HA / C electrolyte powder. (a), (b), (c) and (d) are TEM images of the sample at different magnifications. DETAILED DESCRIPTION
[0034] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0035] Example 1
[0036] The Sn-HA / C negative electrode material was synthesized by hydrothermal method. The specific steps are as follows:
[0037] Take 2.5g humic acid and dissolve it in 50ml 0.5mol·L -1In NaOH solution, gently heat to 60°C on a magnetic stirrer and stir for 1h until humic acid is completely dissolved in the NaOH solution; then add 1.0g of SnO2 to the solution and continue stirring for 1h, then transfer the mixed solution to a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal synthesis reactor, move the reactor to a vacuum drying oven and heat at 120°C overnight (12h), after the reaction is completed, transfer the mixture to a 100ml beaker and continue stirring and heating on a magnetic stirrer to evaporate the solvent, evaporate until the solvent is almost dried, transfer it to a 50ml centrifuge tube and centrifuge it at 2000rpm for 5min, put the obtained solid into a vacuum oven at 80°C and dry it for 12h (overnight), and grind it into a solid powder.
[0038] The solid powder was activated by calcining at 500°C in a tubular furnace under N2 atmosphere for 2 hours. After activation, it was rinsed with deionized water until neutral. The washed product was then dried in a vacuum oven at 80°C for 10 hours (overnight). The obtained material was named Sn-HA / C and used as the negative electrode material of the battery.
[0039] The prepared Sn-HA / C negative electrode material was tested by scanning electron microscopy (SEM), and the results are shown in Figure 1 .from Figure 1 Observation of (a) and (b) shows that most of the products are multi-layered flake structures with an average particle size of 10.0 μm and are relatively dense. Figure 1 (c) and (d) show that the product surface is smooth but still has pores and is slightly curved. It is believed that increasing the sintering temperature can form a denser layered structure, which is beneficial to preventing the volume expansion of Sn particles.
[0040] Example 2
[0041] Hydrothermal synthesis of Na 0.6 Ni 0.8 Co 0.6 O2 positive electrode material, the method is as follows:
[0042] ① Pretreatment of electroplating sludge
[0043] Electroplating sludge was dried in a vacuum oven at 80°C in advance, 2.0 g of dry sludge was soaked in 50 ml of deionized water for 10 min, and then 10 mL of 3 mL -1100g of concentrated hydrochloric acid was added and stirred on a magnetic stirrer for 6 hours until a uniform solution was obtained; next, the pH value of the solution was measured and sodium bicarbonate solution was added to adjust the pH of the solution to neutral. Then 3.6g of urea was added to the above solution and stirred for 30 minutes. The solution was then sealed in a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal synthesis reactor and reacted at 120°C for 12 hours. The obtained mixture was transferred to a 50ml centrifuge tube and centrifuged at 2000rpm for 5 minutes. The solid was dried in an oven at 80°C for 12 hours to obtain a solid powder.
[0044] ② Preparation of nickel-cobalt (Na 0.6 Ni 0.8 Co 0.6 O2) cathode material
[0045] NaHCO3 and CoCl4 with excess sodium in stoichiometric amount and the solid powder obtained in step ① were dissolved in 30 mL of deionized water to form an aqueous solution; sodium oxalate solution was used as a precipitant, 6.5 g of sodium oxalate was used in 1 g of sodium hydroxide solution, and the sodium oxalate solution was slowly added to the aqueous solution under stirring. The final sodium and cobalt contents in the positive electrode material were greater than 62.28 mg / g Na and 55.62 mg / g Co, respectively.
[0046] The resulting mixture was then transferred to a stainless steel hydrothermal synthesis reactor lined with polytetrafluoroethylene, and stirred at 120°C for 12 h (overnight). After the reaction was completed, the solvent was evaporated to remove the solvent. When the solvent was almost evaporated to dryness, it was transferred to a 50 ml centrifuge tube and centrifuged at 2000 rpm for 5 min to obtain a solid precursor. The precursor was calcined at 500°C in a tubular furnace under N2 atmosphere for 2 h to obtain the product Na 0.6 Ni 0.8 Co 0.6 O2 is used as the positive electrode material.
[0047] The prepared Na 0.6 Ni 0.8 Co 0.6 The O2 cathode material was tested by scanning electron microscopy (SEM). The results are shown in Figure 2 .from Figure 2 (a) and (b) show that the product particles are uniform in size and have good aggregation effect. Figure 2 (c) and (d) show that there are still many pores between the particles, indicating that the structure of the synthesized product is not dense enough, which affects the transmission and storage of ions. Increasing the sintering temperature is conducive to forming a denser structure.
[0048] Example 3
[0049] Preparation of Na3Zr2Si2PO 12 -HA / C solid electrolyte, the method is as follows:
[0050] (1) 8 g and 48 g of NaNO3 and ZrOCl2·8H2O in a stoichiometric ratio of 1:2.8 were added to a certain amount of deionized water until they were completely dissolved, and an appropriate amount of nitric acid was added to make the solution pH = 1. Then, 12 g of (NH4)2HPO4 was added to the solution under stirring conditions, and the entire solution became a mixture of colloidal sol and a precipitate of a complex zirconium phosphate compound. The mixture was transferred to a 250 ml conical flask and shaken on a shaker for 12 h (overnight) to allow the mixture to react fully.
[0051] Then the whole mixture was placed in an oven and dried at 120°C for 12 hours to obtain a dry solid powder; the dry solid powder was calcined at 500°C for 2 hours in a tube furnace under a N2 atmosphere to obtain a precursor powder; then 2.5 g and 125 g of SiO2 and humic acid were added to the precursor powder in a corresponding stoichiometric ratio of 1:5, respectively, and the mixture was fully ground and calcined at 500°C for 2 hours in a tube furnace under a N2 atmosphere to obtain the product Na3Zr2Si2PO 12 / HA-C, as the electrolyte material.
[0052] Na3Zr2Si2PO 12 -The conductivity of HA / C electrolyte material is 1589-2734us·cm -1 .
[0053] Figure 3 It is sintered Na3Zr2Si2PO 12 -SEM image of HA / C electrolyte powder, Figure 3 (a) A wide range of particle aggregates of different sizes can be observed, magnified 4,000 times. Figure 3 (b) In the area shown in the picture, a graphene-like layered structure can be clearly observed. The carbonization degree of humic acid in the area is good, and the expected layered structure is generated. The image is further magnified by 20,000 times. Figure 3 (c) and Figure 3 (d) From the structural cross section in the figure, it can be found that the structure has a clear layered structure, and tiny powder particles are attached to its surface. Combined with XRD spectrum analysis, it shows that Na3Zr2Si2PO 12 -HA / C electrolyte was basically synthesized successfully.
[0054] In order to observe the structure of the sample, transmission electron microscopy was used to further characterize it. Figure 4 It is sintered Na3Zr2Si2PO 12 - TEM image of HA / C electrolyte powder. Figure 4As shown in (a), the darker colored area has good conductivity, while the lighter colored area has poor conductivity. The XRD spectrum shows that the conductive part is Na3Zr2Si2PO 12 The NASCION structure is mainly composed of stoichiometric ratios. Figure 4 As shown in (b), crystal agglomeration occurs in some areas, and the surrounding areas are accompanied by pore structures generated by sintering. Although the existence of pore structures may help reduce the impact of volume changes, according to Figure 4 (b) and Figure 4 As shown in (c), the sintered pore area seems to be more prone to agglomeration, which obviously has an adverse effect on the conductivity of the electrolyte; further zooming in, such as Figure 4 (d) Na3Zr2Si2PO 12 The particles have a thin carbon coating layer. Combined with the SEM image results, the overall results show that Na3Zr2Si2PO4 is basically successfully synthesized. 12 -HA / C structure.
[0055] Example 4
[0056] In the Na prepared in Example 1-3 0.6 Ni 0.8 Co 0.6 O2 positive electrode material, Sn-HA / C negative electrode material and Na3Zr2Si2PO 12 -HA / C solid electrolyte materials are added with conductive adhesive poly (vinylidene fluoride-hexafluoropropylene) respectively. The amount of conductive adhesive added to the three materials is 6.5%, 5.5% and 3.5% respectively to achieve a strong bonding effect.
[0057] Then, the negative electrode material, electrolyte material, and positive electrode material containing a conductive binder are pressed into sheets in turn. Specifically, first take an appropriate amount of negative electrode powder (just enough to be evenly spread on the mold surface and not too thick or too thin) and pour it into the mold so that the powder is evenly spread on the surface, and press the tablets at a pressure of 4Mp for 20s; then continue to fill the mold with solid electrolyte powder, press the tablets at a pressure of 4Mp for 20s; then continue to fill the positive electrode powder, and press the tablets at a pressure of 5Mp for 20s.
[0058] In the two-step tableting process of the negative electrode and solid electrolyte, a pressure of 4Mp can be used for tableting. Finally, a pressure of 5Mp is used when the three materials are tableted together. This can avoid excessive pressure on the materials during tableting, which may cause deformation and breakage during the tableting process. It can also avoid the problem of insufficient pressure during tableting, which may cause the powder to fail to form a tablet.
[0059] When slicing, wrap both sides of the electrode with weighing paper (to prevent powder from falling off), and the slice diameter is 14mm (diaphragm 19mm).
[0060] The solid-state battery was assembled in the order of negative electrode shell, shrapnel, gasket, negative electrode sheet, electrolyte sheet, positive electrode sheet and positive electrode shell, and tested after standing for 24 hours.
[0061] The test results show that the voltage of the prepared solid-state battery can reach 2.36V, the current is 9.87mA, and the specific capacity is 736mAh / g. The capacity retention rate is 87% when comparing the capacity of the battery in the first cycle with that in the 50th cycle, and 93% when comparing the capacity of the battery in the fifth cycle with that in the 50th cycle.
[0062] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a solid-state energy storage battery using electroplating sludge and humic acid, characterized in that: Here are the steps: S1. Preparation of Na by hydrothermal synthesis using electroplating sludge as raw material 0.6 Ni 0.8 Co 0.6 O2 cathode material; S2, using humic acid and SnO2 as raw materials to prepare Sn-HA / C negative electrode material by hydrothermal synthesis method; S3. Preparation of Na3Zr2Si2PO4 by solution-assisted solid phase reaction 12 -HA / C solid electrolyte material; the method is as follows: S31, adding NaNO3 and ZrOCl2·8H2O to deionized water, adding nitric acid to make the solution pH = 1, and then adding (NH4)2HPO4 to the solution under stirring conditions, the whole solution becomes a mixture of colloidal sol and a precipitate of a complex zirconium oxyphosphate compound; shaking the mixture on a shaker for 12 hours to allow the mixture to react fully; S32, drying the mixture obtained in step S31 to obtain a solid powder, and calcining the solid powder at 500° C. for 2 h under a N2 atmosphere to obtain a precursor powder; S33, add SiO2 and humic acid to the precursor powder, grind it thoroughly, and calcine it at 500℃ for 2h in N2 atmosphere. The obtained product is Na3Zr2Si2PO 12 / HA-C solid electrolyte material; S4. In Na 0.6 Ni 0.8 Co 0.6 O2 positive electrode material, Sn-HA / C negative electrode material and Na3Zr2Si2PO 12 - Add conductive adhesive to HA / C solid electrolyte materials respectively; S5. The negative electrode material, electrolyte material and positive electrode material containing a conductive adhesive are pressed into sheets in sequence, and then assembled into a solid-state energy storage battery or capacitor in combination with corresponding accessories.
2. The method for preparing a solid-state energy storage battery using electroplating sludge and humic acid as claimed in claim 1, characterized in that: The specific preparation steps of step S1 are as follows: S11, pretreatment of electroplating sludge: adding the dried sludge into deionized water and soaking for 8-12 minutes, then adding hydrochloric acid and stirring to obtain a uniform solution; adjusting the pH of the solution to neutral, then adding urea and stirring to dissolve, sealing the solution in a hydrothermal synthesis reactor, reacting at 110-130° C. for 12 hours, centrifuging the obtained mixture, and drying the filter residue to obtain a solid powder; S12, dissolving NaHCO3 and CoCl4 and the solid powder obtained in step S11 in deionized water, adding sodium oxalate as a precipitant, and then transferring the obtained mixed solution to a hydrothermal synthesis reactor, and reacting at a constant temperature of 110-130°C for 12-14h. After the reaction is completed, evaporating and removing the solvent to obtain a precursor, and calcining the precursor at 500°C for 2-3h under N2 atmosphere to obtain the product Na 0.6 Ni 0.8 Co 0.6 O2 is the positive electrode material.
3. The method for preparing a solid-state energy storage battery using electroplating sludge and humic acid as claimed in claim 1, characterized in that: The specific preparation steps of step S2 are as follows: S21, dissolving humic acid in NaOH solution, adding SnO2 to the solution, stirring evenly, then transferring the mixed solution to a hydrothermal synthesis reactor, moving the reactor to a vacuum drying oven and reacting at 120° C. for 12 h, and evaporating and removing the solvent after the reaction to obtain a solid powder; S22. The solid powder was activated by calcining at 500°C for 2 h in a N2 atmosphere. After activation, it was rinsed with deionized water until neutral and dried. The obtained material was named Sn-HA / C and used as the negative electrode material of the battery.
4. The method for preparing a solid-state energy storage battery using electroplating sludge and humic acid as claimed in claim 3, characterized in that: The mass ratio of humic acid to SnO2 is 5:
2.
5. The method for preparing a solid-state energy storage battery using electroplating sludge and humic acid as claimed in claim 3, characterized in that: In step S21, the method of dissolving humic acid in NaOH solution is: adding humic acid to a concentration of 0.5 mol·L -1 The NaOH solution was heated to 60°C and stirred at a constant temperature until the humic acid was completely dissolved in the NaOH solution.
6. The method for preparing a solid-state energy storage battery using electroplating sludge and humic acid as claimed in claim 1, characterized in that: The conductive adhesive is poly(vinylidene fluoride-hexafluoropropylene), and the added amount accounts for 0.3-5% of the mass of the electrode material or the electrolyte material.
7. The method for preparing a solid-state energy storage battery using electroplating sludge and humic acid as claimed in claim 1, characterized in that: Step S5, preparation method of tableting: first pour the negative electrode powder into the mold to spread the powder evenly on the surface, and press the tablet at a pressure of 4Mp for 20s; then continue to fill the solid electrolyte powder into the mold, and press the tablet at a pressure of 4Mp for 20s; then continue to fill the positive electrode powder, and press the tablet at a pressure of 5Mp for 20s.