A redox artificial synaptic device and preparation method thereof

By designing redox artificial synaptic devices, using redox reactions to regulate PEDOT:PSS resistance state, high dynamic range and multiple plasticity simulation capabilities are achieved, solving the problem of insufficient dynamic range of artificial synaptic devices in the prior art, and improving the The accuracy and computing speed of the neuromorphic computing system are realized.

CN118660618BActive Publication Date: 2024-11-15UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411126534.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-15
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The dynamic range of existing artificial synaptic devices is insufficient, which limits the accuracy and computing speed of neuromorphic computing systems.

Method used

A redox artificial synaptic device was designed, using the structure of ITO bottom electrode, small molecule amine-dedoped PEDOT: PSS resistive layer, solid electrolyte layer and top active electrode, and the synaptic conductance is regulated through redox reaction. The positive pulse enhancement and negative pulse inhibition of conductance are achieved, and the synaptic conductance is regulated through electrochemical group resistance spectrum, DC I-V test and pulse test.

Benefits of technology

The high dynamic range characteristics were achieved, which promoted the development of redox artificial synapses and demonstrated a variety of short-term plasticity simulation capabilities, such as double-pulse facilitation, spike frequency-dependent plasticity, and spike width-dependent plasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118660618B_ABST
    Figure CN118660618B_ABST
Patent Text Reader

Abstract

The present invention relates to a redox artificial synaptic device and a preparation method thereof. The device structure is, from bottom to top, an ITO bottom electrode, a resistive switching layer, a solid electrolyte and a top active electrode, wherein the resistive switching layer is PEDOT:PSS dedoped with small molecule amines. The present invention is based on an artificial synaptic device constructed based on redox reactions, which realizes the characteristics of enhanced conductivity of positive pulse devices and weakened conductivity of negative pulse devices. And due to the continuous redox reaction, the constructed device realizes the characteristics of a high dynamic range. Using a variety of characterization methods, the regulatory mechanism of the redox reaction in the change of synaptic conductance is explained, which promotes the development of redox artificial synapses. The constructed synaptic device successfully realizes a variety of short-term plasticity simulations, including double pulse facilitation, spike frequency-dependent plasticity, spike width-dependent plasticity, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of microelectronic devices, and in particular relates to a redox type artificial synapse device and a preparation method thereof. Background Art

[0002] With the rapid development of artificial intelligence, the Internet of Things, and machine learning, the existing data throughput has grown exponentially, which has put forward higher requirements on data processing systems. However, the current mainstream computing architecture is the von Neumann architecture, whose biggest defect is that the data storage unit and the data processing unit are separated. The exchange of data between the two will generate huge energy consumption and limit the further improvement of the computing speed. Inspired by the human brain, a neuromorphic computing system was proposed. In the neuromorphic computing system, data processing and storage are realized through artificial synaptic units, while the existing artificial synapses have the problem of insufficient dynamic range, which directly leads to the insufficient accuracy of neuromorphic systems in various applications. Artificial synapses can be divided into several types due to their different working mechanisms. Among them, redox synapses have the advantages of continuously adjustable resistance state and simple preparation process, and have great application potential. Therefore, it is very important to explore new materials and design new device architectures for the research of redox artificial synaptic devices. Summary of the invention

[0003] In order to overcome the problems existing in the prior art, the present invention provides a redox type artificial synaptic device and a preparation method thereof.

[0004] A redox artificial synaptic device, the device structure from bottom to top is: an ITO bottom electrode, a resistive layer, a solid electrolyte layer and a top active electrode, the resistive layer is PEDOT:PSS dedoped with small molecule amines, which realizes conductivity conversion after being electrochemically doped with ions; the solid electrolyte layer is used to provide a lithium source; the top active electrode undergoes a redox reaction with lithium ions of the lithium source.

[0005] According to the above aspects and any possible implementation, an implementation is further provided, wherein the preparation process of the small molecule amine dedoped PEDOT:PSS comprises the following steps:

[0006] B1. Weigh a certain amount of PEDOT:PSS particles, dissolve them in deionized water, and stir them at room temperature for a period of time to obtain a first solution;

[0007] B2. Add a small molecule amine to the first solution and continue stirring at room temperature for a period of time to obtain a second solution;

[0008] B3. Deionized water, dodecylbenzenesulfonic acid, 3-glycidyloxypropyltrimethoxysilane and ethylene glycol were stirred and allowed to stand at room temperature to obtain a surfactant;

[0009] B4. Add a surfactant to the second solution and stir at room temperature to obtain small molecule amine dedoped PEDOT:PSS.

[0010] According to the above aspects and any possible implementation, an implementation is further provided, wherein the small molecule amine includes diethylenetriamine DETA, 2,2'-diamino-N-methyldiethylamine DEMTA, tri(2-aminoethyl)amine TAEA or polyethyleneimine PEI.

[0011] According to the aspects and any possible implementations described above, an implementation is further provided, wherein the thickness of the small molecule amine dedoped PEDOT:PSS is 100nm-2um, the thickness of the electrolyte layer is 10-500μm; and the thickness of the top active electrode is 2-50μm.

[0012] According to the aspects described above and any possible implementation, an implementation is further provided, wherein the solid electrolyte layer includes a polymer matrix and a lithium salt; the polymer matrix includes polyethylene oxide, polyvinyl alcohol and / or polyurethane, and the lithium salt includes lithium bistrifluoromethanesulfonyl imide, lithium chloride and / or lithium perchlorate.

[0013] The present invention also provides a method for preparing an artificial synaptic device, wherein the method is used to prepare the artificial synaptic device, and comprises the following steps:

[0014] S1. Treat the PET / ITO substrate to remove surface impurities;

[0015] S2. applying a PEDOT:PSS solution dedoped with a small molecule amine on a PET / ITO substrate from which surface impurities have been removed, annealing and drying at a first set temperature, and reacting at a second set temperature to finally obtain a dedoped PEDOT:PSS film;

[0016] S3. Dropping the electrolyte solution on the dedoped PEDOT: PSS film, annealing at a first set temperature to obtain an electrolyte film;

[0017] S4. drip-coat a carbon nanotube dispersion on the electrolyte film, and anneal at a first set temperature to obtain an artificial synaptic device, wherein the first set temperature is different from the second set temperature.

[0018] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the first set temperature is 20°C-50°C, and the second set temperature is 120°C.

[0019] According to the above aspects and any possible implementation, an implementation is further provided, wherein the application is performed by spin coating or drop coating, the spin coating parameters are 300-1500 rpm, and the spin coating time is 60-300 s.

[0020] According to the above aspects and any possible implementation, a further implementation is provided, wherein the coating amount of the electrolyte solution is 1-20 μL / mm 2 The coating amount of the carbon nanotube dispersion is 1-20 μL / mm 2 .

[0021] According to the above aspects and any possible implementation, an implementation is further provided, wherein the solvent of the electrolyte solution is one of N,N-dimethylformamide or tetrahydrofuran.

[0022] Beneficial effects of the present invention

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1) The artificial synaptic device constructed based on the redox reaction realizes the characteristics of enhanced conductivity of the positive pulse device and weakened conductivity of the negative pulse device. And due to the continuous redox reaction, the constructed device realizes the characteristics of high dynamic range.

[0025] 2) Using electrochemical impedance spectroscopy, direct current IV testing and pulse testing, the regulatory mechanism of synaptic conductance changes was elucidated, promoting the development of redox artificial synapses.

[0026] 3) The constructed synaptic device successfully realized a variety of short-term plasticity simulations, including paired pulse facilitation, spike frequency-dependent plasticity, spike width-dependent plasticity, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Detailed diagram of the device of Example 2 and Example 5 of the present invention;

[0028] Figure 2 Schematic diagram of the ultraviolet spectra of PEDOT:PSS and dedoped PEDOT:PSS in Example 1;

[0029] Figure 3 This is a schematic diagram of the structure of an artificial synapse device according to Embodiment 2 of the present invention;

[0030] Figure 4 is the voltage pulse characteristic curve of the artificial synaptic device in Example 2;

[0031] Figure 5 It is a schematic diagram of the simulation of the double pulse facilitation (PPF) function of the artificial synaptic device in Example 2;

[0032] Figure 6 The spike frequency-dependent plasticity simulation (SRDP), the spike voltage-dependent plasticity simulation (SVDP) and the spike width-dependent plasticity simulation (SDDP) of the artificial synaptic device of Example 2 are as follows;

[0033] Figure 7 This is a DC characteristic diagram of the artificial synapse device of Example 2 of the present invention;

[0034] Figure 8 It is a schematic structural diagram of the device of the present invention;

[0035] Fig. 9 It is a schematic diagram of the electrochemical impedance spectroscopy test results of the device of the present invention. DETAILED DESCRIPTION

[0036] In order to better understand the technical solution of the present invention, the content of the present invention includes but is not limited to the specific implementation methods below, and similar technologies and methods should be considered within the scope of protection of the present invention. In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments.

[0037] It should be clear that the embodiments described in the present invention are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0039] like Figure 8 As shown, the present invention provides a redox type artificial synaptic device, and the device structure is, from bottom to top: an ITO bottom electrode, a small molecule amine dedoped reduced PEDOT:PSS resistive layer, a solid electrolyte layer and a top active electrode. The artificial synaptic device exhibits positive pulse conductivity enhancement, a reduction reaction at the top active electrode, negative pulse conductivity suppression, and an oxidation reaction at the small molecule amine dedoped PEDOT:PSS. Among them, the function of the ITO bottom electrode is to conduct electrons to promote the resistance state transition of PEDOT:PSS; PEDOT:PSS is the device resistive layer that is electrochemically doped with ions to achieve conductivity conversion; the solid electrolyte layer provides a lithium source; and the top active electrode undergoes a redox reaction with the lithium ions in the electrolyte. As shown Figure 8As shown, when a positive pulse voltage is applied, lithium ions in the electrolyte undergo a reduction reaction with the top active electrode, and the anions in the remaining electrolyte electrochemically dope the bottom electrode resistive switching layer PEDOT:PSS to change it from a reduced state to an oxidized state, and the current of the artificial synaptic device increases; when a negative pulse voltage is applied, lithium ions escape from the top active electrode, and the electrochemically doped resistive switching layer PEDOT:PSS changes from an oxidized state to a reduced state, and the current of the artificial synaptic device decreases. The artificial synaptic device regulates the resistive state transition of PEDOT:PSS through redox reactions, and ultimately achieves a continuous transition of synaptic conductance under voltage pulses; the synapse has an obvious advantage in dynamic range; therefore, due to the use of the resistive switching layer PEDOT:PSS, the artificial synaptic device obtained in the present invention has a gradually increasing conductance state under a positive pulse, and a gradually decreasing conductance state under a negative pulse.

[0040] Among them, the thickness of small molecule amine dedoped PEDOT:PSS is 100nm-2um, and the thickness of the electrolyte is 10-500μm; the thickness of the top active electrode is 2-50μm. The different thicknesses of each functional layer will lead to different rates of each electrochemical reaction process inside the artificial synaptic device, and thus cause the artificial synaptic device to exhibit different synaptic characteristics.

[0041] The preparation process of the small molecule amine dedoped PEDOT:PSS used in the resistive switching layer includes the following steps:

[0042] B1. Weigh a certain amount of PEDOT:PSS particles, which are initially in an oxidized state, dissolve them in deionized water, and stir them at room temperature for a period of time to obtain a first solution;

[0043] B2. Add a small molecule amine to the first solution and continue stirring at room temperature for a period of time to obtain a second solution;

[0044] B3. Deionized water, dodecylbenzenesulfonic acid, 3-glycidyloxypropyltrimethoxysilane and ethylene glycol were stirred and allowed to stand at room temperature to obtain a surfactant;

[0045] B4. Add a surfactant to the second solution and stir at room temperature to obtain a reduced PEDOT:PSS aqueous solution dedoped with small molecule amines. After drop coating or spin coating, dry the solution to obtain resistive layer PEDOT:PSS particles, which have a high initial conductivity value and are beneficial to increasing or decreasing the resistance state of the artificial synaptic device.

[0046] The small molecule amine includes diethylenetriamine DETA, 2,2'-diamino-N-methyldiethylamine DEMTA, tri(2-aminoethyl)amine TAEA or polyethyleneimine PEI.

[0047] The solid electrolyte layer includes a polymer matrix and a lithium salt or a hydrogen ion salt; the polymer matrix includes polyethylene oxide, polyvinyl alcohol and / or polyurethane, the lithium salt includes lithium bis(trifluoromethanesulfonyl imide), lithium chloride and / or lithium perchlorate, the hydrogen ion salt includes but is not limited to bis(trifluoromethanesulfonyl imide), wherein the mass of the salt is 10%-100% of the mass of the polymer matrix.

[0048] As an embodiment disclosed in the present invention, the present invention also discloses a method for preparing an artificial synaptic device, wherein the method is used to prepare the artificial synaptic device, and comprises the following steps:

[0049] S1. Treat the PET / ITO substrate to remove surface impurities;

[0050] S2. drip coating or spin coating of a PEDOT:PSS aqueous solution dedoped with a small molecule amine on a PET / ITO substrate from which surface impurities have been removed, annealing and drying at a first set temperature, and reacting at a second set temperature to finally obtain a dedoped PEDOT:PSS film;

[0051] S3. Dropping the electrolyte solution on the dedoped PEDOT: PSS film, annealing at a first set temperature to obtain an electrolyte film;

[0052] S4. Drop coating or sputtering a material as an active top electrode on the electrolyte film, and annealing at a first set temperature to obtain an artificial synaptic device, wherein the first set temperature is different from the second set temperature.

[0053] Specifically, the preparation method of the present invention is as follows:

[0054] (1) Substrate cleaning: Use a UV-ozone cleaning machine to treat the PET / ITO substrate for 20 minutes. The purpose is to reduce the surface energy of ITO, which is conducive to the spread of the PEDOT solution to the entire surface;

[0055] (2) Preparation of PEDOT:PSS resistive switching layer: spin-coat or drop-coat a PEDOT:PSS aqueous solution doped with small molecule amines on a PET / ITO substrate, heat the film at 40°C for 20 minutes in an atmospheric environment to dry the film, and then heat the film at 120°C for 20 minutes to increase the crystallinity of PEDOT and thus improve the carrier transport efficiency, while allowing PEDOT:PSS to fully react with small molecule amines, ultimately obtaining a semiconductor PEDOT:PSS film with a significant band gap;

[0056] (3) preparing an electrolyte layer: dissolving an electrolyte in N,N-dimethylformamide or tetrahydrofuran solvent, continuously drop-coating the electrolyte solution on the dedoped PEDOT:PSS film, and annealing at a first set temperature to obtain an electrolyte film;

[0057] (4) Continue to drip low-dimensional carbon material aqueous solution or sputter gold on the electrolyte film, and anneal at the first set temperature to obtain the top active electrode.

[0058] The electrolyte matrix includes but is not limited to polyethylene oxide, polyvinyl alcohol, and polyurethane, and the lithium salt includes but is not limited to lithium bis(trifluoromethanesulfonyl)imide, lithium chloride, and lithium perchlorate, wherein the mass of the salt is 10%-100% of the mass of the polymer matrix.

[0059] The top active electrode includes, but is not limited to, carbon nanotubes, graphene, gold, silver, copper, aluminum and other materials that can undergo redox reactions with lithium ions.

[0060] In step (2) of the method of the present invention, the preferred spin coating parameters are 300-1500 rpm and the spin coating time is 60-300 s.

[0061] In step (2) of the method of the present invention, the solvent of the PEDOT:PSS solution is deionized water, which can quickly dissolve PEDOT:PSS to obtain a uniform PEDOT:PSS aqueous solution.

[0062] In step (3) of the method of the present invention, the solvent of the electrolyte solution is one of N,N-dimethylformamide and tetrahydrofuran, which has good solubility in the electrolyte matrix material and can obtain a uniform electrolyte solution, which is convenient for the subsequent preparation of the electrolyte layer.

[0063] In steps (3) and (4) of the present invention, the preferred coating amount of the electrolyte solution is 1-20 μL / mm 2 The preferred coating amount of the carbon nanotube dispersion is 1-20 μL / mm 2 .

[0064] The above method is further configured as follows: the first set temperature is 20-50° C., and the preferred insulation time is 10-20 minutes.

[0065] The above method is further configured as follows: the second set temperature is 120° C., and the preferred reaction time is 20 min.

[0066] The following specific embodiments are used to illustrate:

[0067] The modification of the resistive switching layer PEDOT:PSS is carried out by a solution method, and the preparation process is as follows:

[0068] (1) Weigh 0.0400 g of PEDOT:PSS particles, dissolve them in 4 ml of deionized water, and stir them in a magnetic stirrer at room temperature for 4 h to obtain a dark blue undoped PEDOT:PSS aqueous solution.

[0069] (2) Add 8% 2,2'-diamino-N-methyldiethylamine (DEMTA) to the undoped PEDOT:PSS aqueous solution, and continue stirring in a magnetic stirrer at room temperature for 4 h to obtain a small molecule dedoped PEDOT:PSS aqueous solution.

[0070] (3) Prepare a surfactant by adding 3.9 g of deionized water, 0.1 g of dodecylbenzenesulfonic acid, 1 g of 3-glycidyloxypropyltrimethoxysilane, and 5 g of ethylene glycol in sequence, stirring at room temperature for 4 h. After stirring, let the mixture stand for use.

[0071] (4) Add a surfactant with a mass 10 times that of the PEDOT:PSS particles to the small molecule dedoped PEDOT:PSS aqueous solution, and continue stirring in a magnetic stirrer at room temperature for 4 h. The purpose of adding the surfactant is to improve the contact angle between the PEDOT:PSS solution and the ITO substrate.

[0072] Figure 2 By comparing the UV-visible spectra of 8 wt% DEMTA dedoped reduced PEDOT:PSS particles with those of undoped PEDOT:PSS particles (i.e., the raw material particles added in step (1)), it can be seen that the dedoped PEDOT:PSS has a significant absorption effect on visible light with a wavelength of about 625 nm, while the undoped PEDOT has no absorption peak. The resistivity of the undoped PEDOT:PSS measured by the two-probe method is 2 kΩ / cm, and the resistivity of the small molecule doped PEDOT:PSS is 1 GΩ / cm, which indicates that after small molecule dedoping, PEDOT:PSS is transformed into a semiconductor with a significant band gap, which can absorb visible light with a wavelength of 625 nm, proving that its band gap matches photons of this energy.

[0073] The preparation process of a redox artificial synaptic device is as follows:

[0074] (1) A 4 cm x 4 cm flexible PET / ITO substrate was ultrasonically cleaned with acetone, isopropanol, ethanol, and deionized water for 20 min, respectively, and then naturally dried in air.

[0075] (2) Place the cleaned flexible PET / ITO substrate in a UV-ozone cleaning machine for 20 minutes to remove surface impurities.

[0076] (3) Take 100 μL of the modified PEDOT:PSS solution with a pipette and drop it on the flexible PET / ITO substrate. Spin it at 1000 rpm for 120 s, then place it on a hot plate at 40°C, anneal for 20 min, and cool it to room temperature to obtain a PEDOT:PSS film with a thickness of 200 nm. Heat the hot plate to 120°C and keep it for 15 min to allow PEDOT:PSS to fully react with 2,2'-diamino-N-methyldiethylamine (DEMTA) to obtain a small molecule dedoped PEDOT:PSS film.

[0077] (4) Dissolve 0.1 g polyurethane and 0.01 g LiTFSI in 5 ml DMF and stir under a magnetic stirrer at room temperature until the solution becomes a uniform yellow transparent polyurethane lithium salt solution, which is convenient for the subsequent preparation of the electrolyte layer of the artificial synaptic device;

[0078] (5) 200 μL of polyurethane lithium salt solution was drop-coated on the small molecule dedoped PEDOT:PSS film and dried on a hot plate at 40 °C to obtain a transparent electrolyte layer.

[0079] (6) A 10 μL droplet of carbon nanotube dispersion is applied onto the electrolyte film and dried on a hot plate at 40°C to obtain a carbon nanotube active electrode, thereby obtaining an artificial synaptic device.

[0080] Figure 3 This is the structure of the artificial synaptic device obtained in Example 2 of the present invention. The left sub-figure is the structural layout of the device, and the right sub-figure is a cross-sectional schematic diagram of the device. From top to bottom and corresponding cross-sections are the active top electrode 1 of the carbon nanotube, the lithium salt electrolyte 2 of the polyurethane matrix, the DEMTA dedoped PEDOT:PSS resistive layer 3 and the ITO bottom electrode 4.

[0081] Figure 4 The voltage pulse characteristic curve of the artificial synaptic device is shown in Figure 4. The synapse of the structure of Example 2 was electrically tested using a 4200 semiconductor analysis tester, showing the characteristics of enhanced conductivity under positive pulses and suppressed conductivity under negative pulses. Under positive pulse voltage, the carbon nanotube active electrode of the artificial synaptic device undergoes a reduction reaction, and the dedoped PEDOT:PSS undergoes an oxidation reaction from a reduced state to an oxidized state, resulting in an increase in the conductivity of the artificial synaptic device; under negative pulses, the above process is reversed, and the conductivity of the artificial synaptic device decreases.

[0082] Figure 5 The device was demonstrated to simulate the synaptic double-pulse facilitation function. Under a pulse with an amplitude of 3V, a width of 500μs, and an interval of 10μs, the double-pulse facilitation characteristic reached 116%.

[0083] Figure 6From top to bottom, the simulation of spike frequency-dependent plasticity (SRDP, shown in the upper two sub-figures), spike voltage-dependent plasticity (SVDP, shown in the middle two sub-figures) and spike width-dependent plasticity (SDDP, shown in the lower two sub-figures) of artificial synaptic devices are shown in turn. The SRDP index reached a maximum of 218%, the SVDP index reached 214%, and the SDDP index reached 170%, indicating good synaptic simulation function.

[0084] Figure 7 The device's DC IV characteristic curve is displayed, indicating that the artificial synaptic device also exhibits forward voltage enhancement characteristics under DC IV, and the hysteresis loop proves that the artificial synaptic device has a charge storage effect during operation.

[0085] Figure 8 The working mechanism of the device was demonstrated, indicating that the artificial synaptic device realizes synaptic function through the transformation of the oxidation and reduction states of the resistive layer PEDOT:PSS.

[0086] Fig. 9 This is the electrochemical impedance spectroscopy test result of the device. The semi-arc shows that there is capacitance at the interface when the artificial synaptic device is working. Combined with the performance and mechanism analysis of the artificial synaptic device, it can be confirmed that the capacitance of the artificial synaptic device is obtained through the redox reaction between the active electrode and the electrolyte.

[0087] A redox artificial synaptic device preparation process is as follows:

[0088] (1) A 4 cm × 4 cm flexible PET / ITO substrate was ultrasonically cleaned with acetone, isopropanol, ethanol, and deionized water for 20 min, respectively, and then naturally dried in air.

[0089] (2) Place the cleaned flexible PET / ITO substrate in a UV-ozone cleaning machine for 20 minutes to remove surface impurities.

[0090] (3) Take 100 μL of the modified PEDOT:PSS solution with a pipette and drop it on the flexible PET / ITO substrate. Spin it at 500 rpm for 200 s, then place it on a hot plate at 40°C, anneal for 15 min, and cool it to room temperature to obtain a PEDOT:PSS film with a thickness of 500 nm. Heat the hot plate to 120°C and keep it for 15 min to allow PEDOT:PSS to fully react with 2,2'-diamino-N-methyldiethylamine.

[0091] (4) Dissolve 0.1 g polyethylene oxide and 0.01 g lithium chloride in 5 ml DMF and stir under a magnetic stirrer at room temperature until there is no obvious precipitation in the solution.

[0092] (5) 200 μL of polyethylene oxide lithium salt solution was drop-coated on the small molecule dedoped PEDOT:PSS film and dried on a hot plate at 40 °C to obtain a transparent electrolyte film.

[0093] (6) A 200 μL droplet of carbon nanotube dispersion was applied onto the electrolyte film and dried on a hot plate at 40 °C to obtain a carbon nanotube active electrode. By preparing a thicker active electrode and a PPEDOT:PSS resistive switching layer to increase the capacitance of the artificial synaptic device, a larger conductance change can be achieved.

[0094] The modification of the resistive switching layer PEDOT:PSS is carried out by a solution method, and the preparation process is as follows:

[0095] (1) Weigh 0.0400 g of PEDOT:PSS particles, dissolve them in 4 ml of deionized water, and stir them in a magnetic stirrer at room temperature for 4 h to obtain a blue solution.

[0096] (2) Add 8% diethylenetriamine (DETA) containing PEDOT:PSS particles into the solution and continue stirring in a magnetic stirrer at room temperature for 4 h.

[0097] (3) Prepare a surfactant by adding 3.9 g of deionized water, 0.1 g of dodecylbenzenesulfonic acid, 1 g of 3-glycidyloxypropyltrimethoxysilane, and 5 g of ethylene glycol in sequence, stirring at room temperature for 4 h. After stirring, let the mixture stand for use.

[0098] (4) Add a surfactant with a content of 8% of PEDOT:PSS particles to the solution, and continue stirring in a magnetic stirrer at room temperature for 4 hours. The purpose of adding the surfactant is to improve the contact angle between the PEDOT:PSS solution and the ITO substrate.

[0099] A redox artificial synaptic device preparation process is as follows:

[0100] (1) A 4 cm × 4 cm flexible PET / ITO substrate was ultrasonically cleaned with acetone, isopropanol, ethanol, and deionized water for 20 min, respectively, and then naturally dried in air.

[0101] (2) Place the cleaned flexible PET / ITO substrate in a UV-ozone cleaning machine for 20 minutes to remove surface impurities.

[0102] (3) Take 400 μL of DETA-modified PEDOT:PSS solution with a pipette and drop it on the flexible PET / ITO substrate, then place it on a hot plate at 40°C, anneal for 15 minutes and cool to room temperature to obtain a PEDOT:PSS film with a thickness of 2 μm. Heat the hot plate to 120°C and keep it for 15 minutes to allow PEDOT:PSS to fully react with diethylenetriamine.

[0103] (4) Dissolve 0.1 g polyurethane and 0.01 g lithium perchlorate in 5 ml DMF and stir under a magnetic stirrer at room temperature until the solution becomes a uniform, transparent yellow polyurethane lithium salt solution.

[0104] (5) 200 μL of polyurethane lithium salt solution was drop-coated on the DETA-modified PEDOT:PSS film and dried on a hot plate at 40 °C to obtain a transparent electrolyte layer.

[0105] (6) Using a DC sputtering process, gold is deposited on a polyurethane film to obtain a redox artificial synapse with a gold top electrode, such as Figure 1 As shown in Figure 5 of Example 5, the conductivity of gold is higher than that of carbon tubes (such as Figure 1 Example 2 (subfigure) is better, indicating that artificial synaptic devices can achieve conductance conversion at shorter pulse durations.

[0106] The present invention designs a PEDOT:PSS resistive layer, a polymer electrolyte and an active electrode layer. During the preparation process, the thickness of the PEDOT:PSS layer, the concentration of the electrolyte lithium salt and the selection of different active electrodes are controlled to study the optimal synaptic process parameters to promote the development of redox neuromorphic devices.

[0107] The above description shows and describes several preferred embodiments of the present invention, but as mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not depart from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A redox artificial synaptic device, characterized in that: The device structure is, from bottom to top, an ITO bottom electrode, a resistive switching layer, a solid electrolyte layer and a top active electrode, wherein the resistive switching layer is PEDOT:PSS dedoped with small molecule amines, and is electrochemically doped with ions to achieve conductivity conversion; the solid electrolyte layer is used to provide a lithium source; the top active electrode undergoes an oxidation-reduction reaction with lithium ions of the lithium source, and when the lithium ions are reduced in the top active electrode, the PEDOT:PSS dedoped with small molecule amines is doped and oxidized by the remaining anions in the solid electrolyte, and the artificial synaptic device exhibits positive pulse conductivity enhancement; when the reduced lithium ions in the top active electrode are oxidized and combined with the anions in the solid electrolyte, the PEDOT:PSS dedoped with small molecule amines is reduced, and the artificial synaptic device exhibits negative pulse conductivity suppression; The preparation process of the small molecule amine dedoped PEDOT:PSS comprises the following steps: B1. Weigh a certain amount of PEDOT:PSS particles, dissolve them in deionized water, and stir them at room temperature for a period of time to obtain a first solution; B2. Add a small molecule amine to the first solution and continue stirring at room temperature for a period of time to obtain a second solution; B3. Deionized water, dodecylbenzenesulfonic acid, 3-glycidyloxypropyltrimethoxysilane and ethylene glycol were stirred and allowed to stand at room temperature to obtain a surfactant; B4. Add a surfactant to the second solution and stir at room temperature to obtain small molecule amine dedoped PEDOT:PSS.

2. The artificial synaptic device according to claim 1, characterized in that: The small molecule amine includes diethylenetriamine DETA, 2,2'-diamino-N-methyldiethylamine DEMTA, tri(2-aminoethyl)amine TAEA or polyethyleneimine PEI.

3. The artificial synaptic device according to claim 1, characterized in that: The thickness of the PEDOT:PSS dedoped with small molecule amine is 100nm-2um, the thickness of the electrolyte layer is 10-500μm; and the thickness of the top active electrode is 2-50μm.

4. The artificial synaptic device according to claim 1, characterized in that: The solid electrolyte layer includes a polymer matrix and a lithium salt; the polymer matrix includes polyethylene oxide, polyvinyl alcohol and / or polyurethane, and the lithium salt includes lithium bis(trifluoromethanesulfonyl)imide, lithium chloride and / or lithium perchlorate.

5. A method for preparing an artificial synaptic device, characterized in that: The method is used to prepare the artificial synapse device according to any one of claims 1 to 4, comprising the following steps: S1. Treat the PET / ITO substrate to remove surface impurities; S2. applying a PEDOT:PSS solution dedoped with a small molecule amine on a PET / ITO substrate from which surface impurities have been removed, annealing and drying at a first set temperature, and reacting at a second set temperature to finally obtain a dedoped PEDOT:PSS film; S3. Dropping the electrolyte solution on the dedoped PEDOT: PSS film, annealing at a first set temperature to obtain an electrolyte film; S4. drip-coat a carbon nanotube dispersion on the electrolyte film, and anneal at a first set temperature to obtain an artificial synaptic device, wherein the first set temperature is different from the second set temperature.

6. The preparation method according to claim 5, characterized in that: The first set temperature is 20°C-50°C, and the second set temperature is 120°C.

7. The preparation method according to claim 5, characterized in that: The application is performed by spin coating or drop coating, the spin coating parameters are 300-1500 rpm, and the spin coating time is 60-300 s.

8. The preparation method according to claim 5, characterized in that: The coating amount of the electrolyte solution is 1-20 μL / mm 2 The coating amount of the carbon nanotube dispersion is 1-20 μL / mm 2 .

9. The preparation method according to claim 5, characterized in that: The solvent of the electrolyte solution is one of N,N-dimethylformamide and tetrahydrofuran.