A green, low-carbon, fast-reinforced repair concrete and its preparation process

Through green, low-carbon rapid reinforcement and repair concrete composed of sulfaluminate cement, silicate cement, etc., the problem of long construction time and waste of resources of cement concrete repair materials is solved, and the problem of long construction time and waste of resources is achieved through the use of steel slag aggregate and materials such as VAE emulsion. It has efficient and environmentally friendly rapid repair results, meeting the needs of transportation recovery and resource utilization.

CN118666553BActive Publication Date: 2024-12-03SHANDONG JIAOTONG UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411171738.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing cement concrete repair materials have a long construction time, low adhesion force, and it is difficult to quickly restore traffic. The steel slag resources have not been effectively utilized, resulting in environmental pollution and waste of resources.

Method used

Green low-carbon rapid reinforcement and repair concrete composed of sulfur aluminate cement, silicate cement, ultrafine powder, steel slag aggregate and VAE emulsion, etc., through the aging of steel slag aggregate and mineral fibers, combined with lithium-based Accelerator and gypsum retarder adjust the early strength and working properties of concrete to form high-performance rapid repair materials.

Benefits of technology

It has achieved working performance of more than 15 minutes, with a compressive strength of more than 30MPa in one hour and a compressive strength of more than 55MPa in 28 days. It has high early strength, frost resistance and sulfate corrosion resistance, significantly shortens the construction period, saves time, and adopts A large amount of smelting steel slag and recycled aggregates of construction waste have comprehensive benefits of green, low-carbon, energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118666553B_ABST
    Figure CN118666553B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of concrete, and relates to a green low-carbon rapid reinforcement and repairing concrete and a preparation process thereof, wherein the green low-carbon rapid reinforcement and repairing concrete comprises 15-20 parts of sulphoaluminate cement, 12-17 parts of silicate cement, 10-15 parts of ultrafine powder, 25-20 parts of steel slag coarse aggregate or recycled coarse aggregate of construction waste, 9-14 parts of steel slag fine aggregate, 0.05-0.1 parts of water reducer, 2-5 parts of polyvinyl alcohol, 3-7 parts of VAE emulsion, 0.001-0.003 parts of lithium-based coagulant, 0.02-0.05 parts of mineral fiber, 0.02-0.05 parts of gypsum retarder, 0.05-0.1 parts of defoamer, and 10-15 parts of water. The green low-carbon rapid reinforcement and repairing concrete of the present invention is a non-toxic, pollution-free, green and environmentally friendly functional concrete for rapid repair and rapid traffic, with stable product quality and simple on-site construction operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of concrete, and in particular relates to a green, low-carbon, fast-reinforced and repaired concrete and a preparation process thereof. Background Art

[0002] Cement concrete is one of the most widely used man-made structural materials in modern times. It is common for cement concrete buildings to be damaged due to various reasons during their use. According to incomplete statistics, 30%-50% of the existing cement concrete pavements or asphalt pavements will face repair and reinforcement, requiring partial removal and replacement of slabs.

[0003] At present, ordinary Portland cement concrete is still used for local concrete replacement, and its curing time is as long as 14 days. Even with special measures, it takes 7 days to open to traffic. This method has the disadvantages of long construction time, low adhesion to the original cement concrete, and easy falling off. When repairing or renovating the pavement of highways and municipal engineering projects, it is necessary to minimize the impact of construction on traffic. The key to reducing the impact of road repairs on traffic lies in the time it takes for the strength of the repair and reinforcement materials to reach the requirements for traffic or normal operation. Chinese invention patent CN107721328A discloses a rapid traffic repair material and construction method for local replacement of cement concrete pavement. The repair material involved in the invention can meet the requirement of opening to traffic 12 hours after construction, but for sections with large traffic volume and urgent need to resume traffic, the time to open to traffic is still relatively long.

[0004] As steel production increases, the amount of steel slag also increases significantly. The discharge of a large amount of waste not only causes a waste of resources, but also occupies land, pollutes the environment, and seriously restricts economic development. If steel slag is used in the field of ready-mixed concrete, it can not only reduce the cost of concrete, but also be conducive to the high-value-added recycling of steel slag and the research and development of green concrete. It has good social, economic and environmental benefits, and meets the requirements of our country's medium- and long-term scientific and technological development plan. Rapid repair materials have a large number of applications in my country's infrastructure construction concrete projects, such as high-speed railways, highways, water conservancy, oil wells, subways, underground passages and other tunnels and mine construction projects. Therefore, it is a general trend to develop a green and low-carbon rapid reinforcement and repair concrete. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a green, low-carbon, rapid reinforcement and repair concrete and a preparation process thereof, and promotes the development and research of energy-saving, environmentally friendly, high-performance new reinforcement and repair materials. The specific technical scheme is as follows:

[0006] The first object of the present invention is to provide a green, low-carbon, fast-strengthening and repairing concrete, which comprises the following components in parts by weight:

[0007] 15-20 parts of sulphoaluminate cement, 12-17 parts of silicate cement, 10-15 parts of ultrafine powder, 25-20 parts of steel slag coarse aggregate or recycled coarse aggregate from construction waste, 9-14 parts of steel slag fine aggregate, 0.05-0.1 parts of water reducer, 2-5 parts of polyvinyl alcohol, 3-7 parts of VAE emulsion, 0.001-0.003 parts of lithium-based accelerator, 0.02-0.05 parts of mineral fiber, 0.02-0.05 parts of gypsum retarder, 0.05-0.1 parts of defoamer, and 10-15 parts of water;

[0008] The particle size of the steel slag coarse aggregate or the recycled coarse aggregate from construction waste is 5-10 mm; the particle size of the steel slag fine aggregate is 0.075-5 mm; the steel slag coarse aggregate and the steel slag fine aggregate are subjected to aging treatment.

[0009] The recycled coarse aggregate from construction waste is the aggregate obtained by crushing discarded concrete blocks generated from building (structure) demolition, road renovation, concrete production, engineering construction and other situations.

[0010] The green and low-carbon rapid reinforcement and repairing concrete of the present invention can maintain workability for more than 15 minutes and has relatively high early strength, with a 1h compressive strength greater than 30MPa and a flexural strength greater than 4.5MPa. The later strength increases steadily, with a 1d compressive strength greater than 40MPa and a flexural strength greater than 5.5MPa, a 28d compressive strength greater than 55MPa and a flexural strength greater than 8MPa, and has the properties of no volume shrinkage, good frost resistance, sulfate corrosion resistance, excellent adhesion, etc.; it is suitable for the maintenance and reinforcement of bridges, roads, hydraulic engineering and other projects, can greatly shorten the construction period and save time, and also adopts a large amount of smelting steel slag, construction waste recycled aggregates, etc., with significant comprehensive benefits such as green and low-carbon, energy-saving and environmental protection, and high cost performance.

[0011] In the green, low-carbon, fast-reinforced and repaired concrete of the present invention, sulphoaluminate cement enables the concrete to obtain higher mechanical strength in a shorter time after molding to meet the requirements for traffic, and has the characteristics of low raw materials, energy-saving and environmentally friendly production process compared with ordinary cement, high early strength, good frost resistance, strong sulfate corrosion resistance, etc.; silicate cement can improve the later strength, and after compounding with sulphoaluminate cement, it ensures the performance while improving the cost performance; the ultrafine powder has a coupling effect in an alkaline environment, fully utilizing the synergistic effect of various solid wastes, fully releasing their potential to provide silicon (aluminum) tetrahedrons, and greatly reducing the amount of cement used. At the same time, the ultrafine powder also has a ball effect and a filling effect, so that the workability and compactness of the concrete are improved; the aged steel slag aggregate not only has good stability, strength, firmness, good wear resistance, etc., but can also replace natural crushed stone , river sand, saving natural resources, and making full use of the characteristics of steel slag. The potential activity on the surface can produce weak expansion characteristics through volcanic ash reaction, double salt effect, etc., which can replace the expensive and high-carbon emission expansion agent, thereby reducing the shrinkage and cracking of concrete; VAE emulsion has good mechanical properties, the average particle size of the emulsion particles is small, there is a good balance between creep resistance and heat sealing, it has good wet viscosity, fast curing speed and wide bonding performance; the molecular chain of polyvinyl alcohol combines with the cement hydration product (such as calcium aluminate) after cement hydration to form an interface layer, and finally forms a composite structure in which the polymer and the cement hydration are cross-linked, densely filled and interpenetrated, making the system hard and dense with a certain toughness, thereby greatly improving the mechanical properties of the binder; some small grains in the gypsum retarder can be wrapped on the surface of the cement clinker particles and interact with the Ca in the slurry 2+ The reaction forms a dense protective film layer, which can effectively inhibit the hydration reaction and delay the cement setting time within the expected time period; the lithium-based accelerator releases the retarding effect within the expected time period, promotes cement hydration, obtains higher early strength, significantly increases the early strength of the slurry, and significantly shortens the workability time of cement; the synergistic effect of the three admixtures of water reducer, retarder and accelerator can effectively adjust the workability, early strength and workability time of concrete, and provide the required performance for rapid repair and reinforcement.

[0012] Furthermore, the green low-carbon rapid reinforcement and repairing concrete comprises the following components in parts by weight:

[0013] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of superfine powder, 25 parts of steel slag coarse aggregate or recycled coarse aggregate from construction waste, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0014] Furthermore, the mineral fiber is basalt fiber.

[0015] Basalt fiber is a typical silicate fiber. It is easy to disperse when mixed with cement concrete and mortar, making the green, low-carbon, rapid reinforcement and repair concrete stable in volume, easy to work with, and durable. It has excellent temperature resistance, anti-seepage and crack resistance, and impact resistance. It plays a role in reinforcement, anti-seepage and crack resistance, and extending the service life of buildings in construction fields such as houses, bridges, highways, high-speed railways, urban elevated roads, airport runways, seaports, subway tunnels, coastal protection projects, nuclear power plant facilities, and military facilities.

[0016] Furthermore, the silicate cement is a composite of one or two of silicate cement, ordinary silicate cement, pozzolanic silicate cement, fly ash silicate cement and slag silicate cement.

[0017] Calcium hydroxide, the hydration product of silicate cement, can promote the dissolution and activation of active ingredients in geopolymers such as active silica and alumina, and react with them to form more stable hydration products, such as calcium aluminate hydrate, calcium silicate hydrate, ettringite AFt, as well as zeolite phases, sodium aluminochlorate and other crystal structures, which form a dense three-dimensional network system structure, thereby enhancing the overall performance of the concrete system.

[0018] Furthermore, the specific surface area of ​​the ultrafine powder is 500-600m 2 / kg.

[0019] If the ultrafine powder is too coarse, it will not play a filling role and the reinforcing effect will be poor; if the ultrafine powder is too fine, the cost will be high and the reinforcing effect will not be obvious.

[0020] Furthermore, the ultrafine powder comprises the following components in parts by weight: 40-45 parts of fly ash, 40-50 parts of blast furnace slag powder, 5-7 parts of desulfurized gypsum, and 6-10 parts of silicon powder.

[0021] Furthermore, the steel slag coarse aggregate and the steel slag fine aggregate are hot-stewed steel slag aged and stored for at least 6 months.

[0022] Furthermore, the fineness modulus of the steel slag fine aggregate is 2.7-3.2.

[0023] Furthermore, the water reducing agent has a water reducing rate of ≥20%.

[0024] Furthermore, the water reducer is any one or more of a polycarboxylate water reducer, a naphthalene-based water reducer, and an aminosulfonate water reducer.

[0025] Furthermore, the VAE emulsion is one of VAE707 emulsion, VAE705 emulsion and VAE806 emulsion.

[0026] Furthermore, the lithium-based coagulant is a mixture of lithium carbonate and lithium silicate, and the mass ratio of the lithium carbonate to the lithium silicate is 7:3.

[0027] The second object of the present invention is to provide a preparation process of the above-mentioned green low-carbon rapid reinforcement and repairing concrete, comprising the following steps:

[0028] Weigh sulphoaluminate cement, silicate cement, ultrafine powder, steel slag coarse aggregate or recycled coarse aggregate from construction waste, steel slag fine aggregate, water reducer, lithium-based accelerator, mineral fiber, gypsum retarder, defoamer, and polyvinyl alcohol in proportion and dry mix for at least 30 seconds, then add a mixed solution of VAE emulsion and water, and stir thoroughly for at least 2 minutes to obtain green, low-carbon, fast-reinforced and repaired concrete.

[0029] The method for using the green low-carbon rapid reinforcement and repairing concrete comprises the following steps:

[0030] S1: Clean and moisten the old concrete interface: remove the mortar from the interface of the old concrete section to expose fresh aggregate and keep the interface moist and clean;

[0031] S2: The mixed green low-carbon rapid reinforcement repair concrete is quickly transported to the pouring site, compacted and smoothed using a vibrating rod combined with a flat plate tamping rod;

[0032] S3: Maintenance: After the surface shaping is completed, cover with film for maintenance or apply curing agent for maintenance for 1 hour before opening to traffic.

[0033] The beneficial effects of the present invention are:

[0034] The green low-carbon rapid reinforcement and repairing concrete of the present invention can maintain workability for more than 15 minutes, and has high early strength, high bonding strength, good flexibility, suitable compressive and flexural strength, low compression-flexural ratio, good wear resistance, good crack resistance, small drying shrinkage value, and good compatibility with cement concrete materials and asphalt mixtures. It is suitable for the repair and reinforcement of bridges, roads, hydraulic engineering and other projects, which can greatly shorten the construction period and save time. The selected raw materials are widely available and low in price. A large amount of industrial waste such as smelting steel slag and construction waste recycled aggregates are also used to replace natural aggregates. It can not only meet the needs of rapid repair and reinforcement of the project, but also expand the comprehensive utilization of steel slag and construction waste recycled aggregates, and has significant comprehensive benefits such as green and low carbon, energy saving and environmental protection, and high cost performance. It can be mixed on site or evenly mixed in a fixed ratio by factory dry-mixed concrete production equipment. The product quality is stable, and the on-site construction operation is simple. After adding water and mixing, it has good workability and water retention. The green low-carbon rapid reinforcement and repairing concrete of the present invention is a non-toxic, pollution-free, green and environmentally friendly functional concrete for rapid repair and rapid traffic opening. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a photo of the test block of the green and low-carbon rapid reinforcement and repair type concrete of Example 1 of the present invention after 1 hour of demolding. DETAILED DESCRIPTION

[0036] The instruments, reagents, materials, etc. involved in the following embodiments, unless otherwise specified, are all conventional instruments, reagents, materials, etc. in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following embodiments, unless otherwise specified, are all conventional experimental methods, detection methods, etc. in the prior art.

[0037] Sulphoaluminate cement: 42.5 grade rapid hardening sulphoaluminate cement (R·SAC) produced by Zhengzhou Jianwen Special Materials Technology Co., Ltd., with a specific surface area greater than 400m 2 / kg, 45μm negative pressure sieve passing rate is 82.1%, 80μm negative pressure sieve passing rate is 98.2%;

[0038] Portland cement: P.O42.5 Portland cement;

[0039] Ultrafine powder: specific surface area is 560m 2 / kg, in parts by weight, including 40 parts of fly ash, 46 parts of blast furnace slag powder, 6 parts of desulfurized gypsum, and 8 parts of silicon powder;

[0040] Steel slag coarse aggregate: hot-stewed steel slag aged for 8 months, with a particle size of 5-10mm;

[0041] Steel slag fine aggregate: hot-stewed steel slag aged for 8 months, with a particle size of 0.075-5mm and a fineness modulus controlled at 2.7-3.2;

[0042] Water reducer: polycarboxylate water reducer.

[0043] VAE (vinyl acetate-ethylene copolymer) emulsion: VAE707 emulsion;

[0044] Lithium-based coagulant: a mixture of lithium carbonate and lithium silicate in a mass ratio of 7:3;

[0045] Mineral fiber: basalt fiber;

[0046] Defoaming agent: Cement mortar defoaming agent produced by Huizhou Huashengyuan New Materials Co., Ltd., model DT1060.

[0047] The above materials were used in the following examples and comparative examples.

[0048] Embodiment 1:

[0049] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0050] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0051] The method for preparing a test block of the green low-carbon rapid reinforcement and repairing concrete comprises the following steps:

[0052] 1. Preparation work, test mold preparation: First, clean the test mold, and then evenly apply the coating agent on the inner surface;

[0053] 2. Use a one-time forced mixer for mixing and pouring to prepare concrete: weigh sulphoaluminate cement, silicate cement, ultrafine powder, steel slag, water reducer, lithium-based accelerator, mineral fiber, gypsum retarder, defoamer, and polyvinyl alcohol in proportion and dry mix for at least 30 seconds, then add a mixed solution of VAE emulsion and water and stir thoroughly for at least 2 minutes to obtain green, low-carbon, rapid reinforcement and repair concrete;

[0054] 3. Put the green low-carbon rapid reinforcement repair concrete into the test mold three times, each time the material is about 1 / 3 of the test mold height, and then use a tamping rod to tamp or a small vibrating rod to vibrate for about 20 seconds until no bubbles are discharged, and so on, until it is completed;

[0055] 4. Cover the assembled cubic test block with film and place it on site for curing for 1 hour. After removing the mold, the test block is Figure 1 .

[0056] The performance test of the green and low-carbon rapid reinforcement and repair concrete is carried out in accordance with the "Test Code for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020), "Standard for Test Methods for Physical and Mechanical Properties of Concrete" (GB / T 50081-2019), "Standard for Test Methods for Basic Performance of Building Mortar" (JGJ / T 70-2009) and "Technical Specifications for Safety Assessment of Engineering Structure Reinforcement Materials" (GB 50728-2011); the result judgment is carried out in accordance with the "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT 1211.1-2018).

[0057] Test results:

[0058] The green low-carbon rapid reinforcement repair concrete prepared in this embodiment has a concrete slump of 175 mm and an initial setting time of 19 min. Figure 1, well-formed, without obvious appearance defects such as bubbles, holes, cracks, etc., 1h compressive strength is 42.5MPa, flexural strength is 5.2MPa; 1d compressive strength is 55.2MPa, flexural strength is 6.7MPa; 28d compressive strength is 62.6MPa, flexural strength is 8.7MPa; 1d bonding strength with benchmark concrete is 1.9MPa, after frost resistance test (freeze 4h, thaw 4h), when the mass loss is 5%, the number of repeated freeze-thaw cycles is 225 times, far greater than 150 times, the compressive strength is 54.1MPa, and the strength loss rate is 7.6%. All the above indicators meet the corresponding model technical requirements of "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT 1211.1-2018).

[0059] The method for using the green low-carbon rapid reinforcement and repairing concrete comprises the following steps:

[0060] S1: Clean and moisten the old concrete interface: remove the mortar from the interface of the old concrete section to expose fresh aggregate and keep the interface moist and clean;

[0061] S2: The mixed green low-carbon rapid reinforcement repair concrete is quickly transported to the pouring site, compacted and smoothed using a vibrating rod combined with a flat plate tamping rod;

[0062] S3: Maintenance: After the surface shaping is completed, cover with film for maintenance or apply curing agent for maintenance for 1 hour before opening to traffic.

[0063] Embodiment 2:

[0064] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0065] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of recycled coarse aggregate from construction waste, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoaming agent, and 12.838 parts of water. The particle size of the recycled coarse aggregate from construction waste is 5-10mm.

[0066] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0067] Test results:

[0068] Compared with Example 1, this embodiment uses recycled coarse aggregate from construction waste instead of steel slag coarse aggregate, and the other components remain unchanged. The prepared green, low-carbon, rapid reinforcement and repair type concrete has a concrete slump of 180 mm and an initial setting time of 20 min. The test block is well formed after demolding for 1 hour, without obvious appearance defects such as bubbles, holes, and cracks. The compressive strength at 1 hour is 41.1 MPa, and the flexural strength is 5.0 MPa; the compressive strength at 1d is 51.6 MPa, and the flexural strength is 6.3 MPa; the compressive strength at 28d is 58.9 MPa, and the flexural strength is 8.5 MPa; the bonding strength between 1d and the benchmark concrete is 1.8 MPa. After the frost resistance test (freezing for 4 hours and thawing for 4 hours), when the mass loss is 5%, the number of repeated freeze-thaw cycles is 240 times, the compressive strength is 54.1 MPa, and the strength loss rate is 8.1%. All the above indicators meet the technical requirements of the corresponding models of "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT1211.1-2018).

[0069] Comparative Example 1:

[0070] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0071] 21 parts of sulphoaluminate cement, 14 parts of silicate cement, 9 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0072] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0073] Compared with the embodiment, the sulphoaluminate cement in this comparative example 1 is increased by 3 parts, and the ultrafine powder is reduced by 3 parts accordingly. After testing, the green low-carbon rapid reinforcement and repair concrete prepared by this comparative example has a slump of 135mm, an initial setting time of only 13min, and a shorter working duration, which no longer meets the technical requirements of the corresponding model of "Rapid Repair Materials for Highway Engineering Cement Concrete Part 1: Cement-based Repair Materials" (JTT 1211.1-2018) that the initial setting time is ≥15min. This is because sulphoaluminate cement is a fast-hardening and early-strength cement. If the initial setting time is extended, a retarder must be added, which not only affects the early strength, but also leads to increased costs.

[0074] Comparative Example 2:

[0075] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0076] 14 parts of sulphoaluminate cement, 14 parts of silicate cement, 16 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0077] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0078] Compared with the embodiment, the amount of sulphoaluminate cement in this comparative example 2 is reduced by 4 parts, and the amount of superfine powder is increased by 4 parts accordingly. After testing, the slump of the green low-carbon rapid reinforcement and repair concrete prepared by this comparative example is 190mm, the initial setting time is 40min, and the 1h compressive strength is only 21.3MPa, which does not meet the strength technical requirements of the corresponding CRRM-I type in "Rapid Repair Materials for Highway Engineering Cement Concrete Part 1: Cement-based Repair Materials" (JTT 1211.1-2018). This is because sulphoaluminate cement is a fast-hardening and early-strengthening cement. Reducing its dosage and increasing the dosage of superfine powder will lead to a decrease in early strength, which can no longer meet the 1h traffic requirements.

[0079] Comparative Example 3:

[0080] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0081] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 27 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 1 part of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0082] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0083] Compared with the embodiment, the amount of polyvinyl alcohol in this comparative example 3 is reduced by 2 parts, and the amount of coarse aggregate is increased by 2 parts accordingly. According to the test, the slump of the green low-carbon rapid reinforcement and repair concrete prepared by this comparative example is 170mm, the initial setting time is 20min, and the test block is well formed after demolding for 1h, without obvious appearance defects such as bubbles, holes, and cracks. The compressive strength is 38.8MPa at 1h, and the flexural strength is 4.4MPa at 1d; the compressive strength is 47.6MPa at 1d, and the flexural strength is 5.0MPa; it can be seen that the flexural strength at 1h and 1d do not meet the strength technical requirements of the corresponding CRRM-I type in "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT1211.1-2018). The main reason is that when the amount of polyvinyl alcohol is small, it cannot be fully cross-linked and filled with calcium aluminate after cement hydration, resulting in reduced mechanical properties, especially affecting its toughness. Therefore, polyvinyl alcohol should be reasonably added, and it shall not be less than the design requirement of 2 parts by mass.

[0084] Comparative Example 4:

[0085] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0086] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 22 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 6 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0087] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0088] Compared with the embodiment, the polyvinyl alcohol in this comparative example 4 is increased to 6 parts, and the coarse aggregate is reduced by 3 parts accordingly. After testing, the slump of the green low-carbon rapid reinforcement and repair type concrete prepared by this comparative example is 175mm, the initial setting time is 21min, and the test block is well formed after demolding for 1h, without obvious appearance defects such as bubbles, holes, and cracks. The compressive strength is 43.1MPa at 1h and the flexural strength is 4.8MPa at 1d; the compressive strength is 51.3MPa at 1d and the flexural strength is 5.7MPa. It can be seen that with the increase of polyvinyl alcohol, its mechanical properties are not increased or improved much relative to the embodiment, but the cost is increased. The main reason is that when the amount of polyvinyl alcohol is large, the coupling effect with calcium aluminate after cement hydration is weakened. Therefore, polyvinyl alcohol should be reasonably added.

[0089] Comparative Example 5:

[0090] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0091] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 27 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 2 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0092] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0093] Compared with the embodiment, the VAE emulsion in this comparative example 5 is reduced by 2 parts, and the coarse aggregate is increased by 2 parts accordingly. After testing, the green low-carbon rapid reinforcement and repair type concrete prepared by this comparative example has a slump of 170mm, an initial setting time of 23min, a 1h compressive strength of 42.1MPa, and a flexural strength of 4.7MPa; a 1d compressive strength of 50.9MPa, and a flexural strength of 5.7MPa; and a 1d bonding strength with the benchmark concrete of 1.36MPa. It can be seen that the 1d bonding strength with the benchmark concrete does not meet the strength technical requirements of the corresponding CRRM-I type in "Rapid Repair Materials for Highway Engineering Cement Concrete Part 1: Cement-based Repair Materials" (JTT 1211.1-2018). The main reason is that VAE emulsion has good wet viscosity and fast curing speed. When the dosage is small, the bonding effect with the original concrete is weakened. Therefore, its dosage should be reasonably controlled.

[0094] Comparative Example 6:

[0095] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0096] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 21 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 2 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

[0097] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0098] In Comparative Example 6, compared with the embodiment, the VAE emulsion is increased to 8 parts, and the coarse aggregate is correspondingly reduced by 4 parts. After testing, the green, low-carbon, fast-reinforced and repaired concrete prepared by this comparative example has a slump of 170 mm, an initial setting time of 28 min, a 1h compressive strength of 39.5 MPa, and a flexural strength of 4.4 MPa; a 1d compressive strength of 48.8 MPa, and a flexural strength of 4.8 MPa; and a 1d bonding strength with the benchmark concrete of 1.51 MPa. It can be seen that the initial setting time is prolonged, resulting in a decrease in the 1h and 1d mechanical properties compared with the embodiment. This is because too much VAE emulsion hinders the hydration of cement. Therefore, its maximum dosage should be reasonably controlled.

[0099] Comparative Example 7:

[0100] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0101] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 2 parts of VAE emulsion, 0 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoaming agent, and 12.84 parts of water.

[0102] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0103] Compared with the embodiment, the amount of lithium-based coagulant added in this comparative example 7 is 0, and the amount of water used is increased accordingly. After testing, the green low-carbon rapid reinforcement and repair type concrete prepared by this comparative example has a slump of 200mm, an initial setting time of 35min, a 1h compressive strength of 27.7MPa, and a flexural strength of 3.0MPa. It can be seen that compared with the embodiment, the initial setting time is prolonged without adding lithium-based coagulant, and the 1h mechanical properties do not meet the strength technical requirements of the corresponding CRRM-I type in "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT 1211.1-2018). This is because the appropriate lithium-based coagulant can accelerate cement hardening in the sulphoaluminate cement system.

[0104] Comparative Example 8:

[0105] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0106] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 2 parts of VAE emulsion, 0.003 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.84 parts of water.

[0107] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0108] Compared with the embodiment, the amount of lithium-based coagulant added in this comparative example 8 is 0, and the water consumption is increased accordingly. After testing, the green and low-carbon rapid reinforcement and repair type concrete prepared by this comparative example has a slump of 135mm, an initial setting time of 13.5min, a 1h compressive strength of 43.7MPa, and a flexural strength of 4.6MPa. It can be seen that, relative to the embodiment, increasing the amount of lithium-based coagulant leads to a shortened initial setting time, and the working duration is too short to be conducive to construction, and the technical requirements of the corresponding CRRM-I type of "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT 1211.1-2018) are not met.

[0109] Comparative Example 9:

[0110] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0111] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.01 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.858 parts of water.

[0112] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0113] Compared with the embodiment, the mineral fiber in this comparative example 9 is reduced to 0.01 parts, and the water is correspondingly increased by 0.02 parts. After testing, the green and low-carbon rapid reinforcement and repair type concrete prepared by this comparative example has a slump of 205mm and an initial setting time of 23min. After demolding for 1h, the test block is well formed without obvious appearance defects such as bubbles and holes. The 1h compressive strength is 41.1MPa and the flexural strength is 4.35MPa; the 1d compressive strength is 48.8MPa and the flexural strength is 5.21MPa. It can be seen that the reduction of mineral fiber cannot share the bending and tensile stress of concrete, resulting in a decrease in the 1h flexural strength compared with the embodiment, which no longer meets the corresponding technical requirements of "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT 1211.1-2018).

[0114] Comparative Example 10:

[0115] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0116] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.06 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.818 parts of water.

[0117] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0118] Compared with the embodiment, the mineral fiber in this comparative example 10 is increased to 0.06 parts, and the water is correspondingly reduced by 0.02 parts. After testing, the green, low-carbon, fast-reinforced and repaired concrete prepared by this comparative example has a slump of 130 mm, an initial setting time of 19 min, and a good test block after demolding for 1 hour without obvious appearance defects such as bubbles, holes, and cracks. The 1-hour compressive strength is 44.1 MPa, and the flexural strength is 5.4 MPa; the 1-day compressive strength is 56.6 MPa, and the flexural strength is 6.7 MPa. It can be seen that with the increase of mineral fiber, the slump is much lower than that of the embodiment, the mechanical indicators are all improved, and the workers are relatively difficult to operate. Therefore, the dosage should be properly controlled.

[0119] Comparative Example 11:

[0120] A green low-carbon rapid reinforcement and repairing concrete, composed of the following components in parts by weight:

[0121] 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of ultrafine powder, 25 parts of steel slag coarse aggregate, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.06 parts of mineral fiber, 0.06 parts of gypsum retarder, 0.02 parts of defoamer, and 12.818 parts of water.

[0122] The method for preparing the test block of the green low-carbon rapid reinforcement and repairing concrete is the same as that in Example 1 and will not be repeated here.

[0123] Compared with the embodiment, the gypsum retarder in this comparative example 11 is increased to 0.06 parts, and the water is correspondingly reduced by 0.02 parts. After testing, the green low-carbon rapid reinforcement and repair type concrete prepared by this comparative example has an increased slump of 220mm, an initial setting time of 35min, and a good test block after demolding after 1h, without obvious appearance defects such as bubbles, holes, and cracks. The 1h compressive strength is 25.6MPa and the flexural strength is 2.8MPa; it does not meet the technical requirements of the corresponding CRRM-I type of "Rapid Repair Materials for Cement Concrete in Highway Engineering Part 1: Cement-based Repair Materials" (JTT 1211.1-2018). Therefore, its dosage should be properly controlled.

[0124] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A green, low-carbon, rapid reinforcement and repair concrete, characterized in that: In parts by weight, it includes the following components: 15-20 parts of sulphoaluminate cement, 12-17 parts of silicate cement, 10-15 parts of ultrafine powder, 20-25 parts of steel slag coarse aggregate or recycled coarse aggregate from construction waste, 9-14 parts of steel slag fine aggregate, 0.05-0.1 parts of water reducer, 2-5 parts of polyvinyl alcohol, 3-7 parts of VAE emulsion, 0.001-0.003 parts of lithium-based accelerator, 0.02-0.05 parts of mineral fiber, 0.02-0.05 parts of gypsum retarder, 0.02 parts of defoamer, 10-15 parts of water; The particle size of the steel slag coarse aggregate or the recycled coarse aggregate from construction waste is 5-10 mm; the particle size of the steel slag fine aggregate is 0.075-5 mm; The mineral fiber is basalt fiber; the ultrafine powder comprises the following components: 40-45 parts of fly ash, 40-50 parts of blast furnace slag powder, 5-7 parts of desulfurized gypsum, and 6-10 parts of silicon powder; The lithium-based coagulant is a mixture of lithium carbonate and lithium silicate; The steel slag coarse aggregate and the steel slag fine aggregate are hot-stewed steel slag that has been aged and stored for at least 6 months.

2. The green, low-carbon, rapid reinforcement and repairing concrete according to claim 1 is characterized in that: In parts by weight, it includes the following components: 18 parts of sulphoaluminate cement, 14 parts of silicate cement, 12 parts of superfine powder, 25 parts of steel slag coarse aggregate or recycled coarse aggregate from construction waste, 11 parts of steel slag fine aggregate, 0.07 parts of water reducer, 3 parts of polyvinyl alcohol, 4 parts of VAE emulsion, 0.002 parts of lithium-based accelerator, 0.03 parts of mineral fiber, 0.04 parts of gypsum retarder, 0.02 parts of defoamer, and 12.838 parts of water.

3. The green, low-carbon, rapid reinforcement and repairing concrete according to claim 1 is characterized in that: The silicate cement is a composite of one or two of silicate cement, ordinary silicate cement, pozzolanic silicate cement, fly ash silicate cement and slag silicate cement.

4. The green, low-carbon, rapid reinforcement and repairing concrete according to claim 1 is characterized in that: The specific surface area of ​​the ultrafine powder is 500-600m 2 / kg.

5. The green, low-carbon, rapid reinforcement and repairing concrete according to claim 1 is characterized in that: The water reducer is any one or more of a polycarboxylate water reducer, a naphthalene-based water reducer, and an aminosulfonate water reducer; and the VAE emulsion is one of a VAE707 emulsion, a VAE705 emulsion, and a VAE806 emulsion.

6. The green, low-carbon, rapid reinforcement and repairing concrete according to claim 5 is characterized in that: The water reducing rate of the water reducing agent is ≥20%, the fineness modulus of the steel slag fine aggregate is 2.7-3.2, and the mass ratio of the lithium carbonate salt to the lithium silicate salt is 7:

3.

7. A process for preparing the green, low-carbon, rapid reinforcement and repairing concrete according to any one of claims 1 to 6, characterized in that: The steps include: Weigh sulphoaluminate cement, silicate cement, ultrafine powder, steel slag coarse aggregate or recycled coarse aggregate from construction waste, steel slag fine aggregate, water reducer, lithium-based accelerator, mineral fiber, gypsum retarder, defoamer, and polyvinyl alcohol in proportion and dry mix for at least 30 seconds, then add a mixed solution of VAE emulsion and water, and stir thoroughly for at least 2 minutes to obtain green, low-carbon, fast-reinforced and repaired concrete.

Citation Information

Patent Citations

  • Quick traffic opening repair material for local plate replacement of cement concrete pavement, and construction method thereof

    CN107721328A

  • Low-temperature quick repair mortar for pavement and preparation method for low-temperature quick repair mortar

    CN102826813A

  • Method for detecting steel-slag stability of full-graded steel-slag concrete

    CN104090091A

  • Concrete pavement repairing material and preparation method and application thereof

    CN109851304A

  • High flowing crack-resistant early strength repair mortar and preparation method thereof