A method for preparing Snoek relaxation type high damping and high plasticity titanium alloy
Through ingot smelting, deformation processing and heat treatment processes, combined with Zr element and gradient high-temperature annealing, the microstructure of titanium alloy is regulated, and the problems of brittle fracture and low plasticity of high damping titanium alloy are solved, achieving both high damping and high plasticity. Effect.
Patent Information
- Application Number
- CN202411154205.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Existing high-damping titanium alloys are prone to brittle fracture during the elastic deformation stage, which limits its engineering application, and the addition of high oxygen content leads to insufficient plastic processing deformation ability of the material.
The microstructure and heterogeneous structure of titanium alloy are regulated by combining ingot smelting, deformation processing and heat treatment processes, and the damping and plastic deformation ability are improved by adding trace Zr elements, gradient high-temperature annealing and rolling deformation.
A high-damping high-plastic titanium alloy with a damping coefficient greater than 0.08 and a uniform elongation of room temperature stretch exceeding 20%, solving the problem of brittle fracture and improving the production efficiency and application range of the material.
Smart Images

Figure CN118668098B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of advanced structural functional integrated materials, and specifically relates to a preparation method of a Snoek relaxation type high-damping high-plasticity titanium alloy. Background Art
[0002] With the development of modern industrial technology, high-power mechanical equipment is increasingly being used in extreme environments. In order to reduce the harmful effects of mechanical vibration and noise on structural safety and living environment, higher requirements are placed on the comprehensive mechanical properties and damping properties of advanced structural functional integrated materials. At present, titanium alloys have attracted extensive attention in basic scientific research and engineering applications due to their low density, high specific strength, corrosion resistance, non-magnetic properties, and excellent functionality. Recently, a high-damping titanium alloy Ti-25Nb-3O (at.%, i.e., Ti-39Nb-0.845Owt.%) based on the Snoek relaxation theory was reported. It produces significant high-damping properties by adding high oxygen content and utilizing interstitial atomic migration relaxation. However, the high-damping alloy suffers from brittle fracture during the elastic deformation stage, which becomes a technical bottleneck that limits its practical engineering application. Therefore, the current problem to be solved is how to further improve the plastic deformation capacity of the alloy while maintaining the existing high damping properties, especially how to obtain high plasticity while maintaining high damping and high strength.
[0003] In recent years, based on the idea of heterogeneous strain hardening, the simultaneous improvement of material strength and plasticity has been achieved in metal structural materials such as high-strength steel, medium-high entropy alloys, aluminum alloys, and high-strength titanium alloys through the regulation of microstructure. With the help of additional strain hardening induced by heterogeneous deformation, it is expected to achieve an improvement in the tensile plasticity of materials in high-damping titanium alloys. However, in the process of heterogeneous microstructure regulation of high-damping titanium alloys, the insufficient plastic processing deformation capacity of materials caused by the addition of high oxygen content is still a problem. Studies have shown that in the allotropic hexagonal close-packed α-Ti and body-centered cubic β-Ti of titanium, oxygen is an α-Ti stabilizing element and has a higher solid solubility in α-Ti. The plastic deformation capacity of high-oxygen content titanium alloys can be further adjusted by regulating the orientation of different hexagonal close-packed textures at high temperature; in addition, the reasonable addition of trace alloying elements can also improve the deformation capacity of titanium alloys. It can be seen that through the strategy of organizational regulation and element distribution, combined with the idea of heterogeneous strain hardening and texture orientation regulation, it is expected to significantly improve the plastic deformation ability of Snoek relaxation type high damping titanium alloy, and then design titanium alloy materials with both high damping and high plasticity. Summary of the invention
[0004] In view of the technical problems existing in the above-mentioned background technology, the present invention proposes a method for preparing a Snoek relaxation type high-damping and high-plasticity titanium alloy. The method has a reasonable concept and utilizes a combination of ingot melting, deformation processing and heat treatment processes to prepare a high-damping and high-plasticity titanium alloy with a damping coefficient greater than 0.08 and a uniform tensile elongation of more than 20% under quasi-static conditions at room temperature. The method can effectively solve the technical bottleneck problem of brittle fracture of high-oxygen content Snoek relaxation type high-damping titanium alloy in the elastic stage in the prior art.
[0005] To solve the above technical problems, the present invention provides a method for preparing a Snoek relaxation type high damping and high plasticity titanium alloy, which mainly comprises the following steps:
[0006] (1) Sponge titanium, pure titanium foil, pure niobium particles, pure zirconium flakes and TiO2 powder are used as raw materials for melting alloys and are proportioned according to a predetermined mass percentage, and then the proportioned raw materials are repeatedly melted in a vacuum melting furnace and naturally cooled in a water-cooled copper crucible in the vacuum melting furnace to obtain a high damping titanium alloy ingot material;
[0007] (2) subjecting the high damping titanium alloy ingot material obtained in the above step (1) to homogenization treatment at a predetermined homogenization treatment temperature and time range and under anti-oxidation protection measures, and then subjecting the homogenization treatment to high temperature forging treatment to obtain a high damping titanium alloy profile blank;
[0008] (3) subjecting the high damping titanium alloy profile blank obtained in the above step (2) to a gradient high temperature annealing treatment within a predetermined temperature and time range and under anti-oxidation protection measures, and then subjecting the primary profile blank to a rolling process with multiple passes of different reductions, and then subjecting the surface of the rolled primary profile blank to a mechanical grinding process and a decontamination process to obtain a high damping titanium alloy material;
[0009] (4) The high damping titanium alloy material obtained in the above step (3) is subjected to an ordered annealing treatment and a cooling treatment within a predetermined temperature and time range to finally obtain a high damping titanium alloy material with a heterogeneous structure.
[0010] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein the element mass percentage of the high damping titanium alloy ingot material in the step (1) is: Nb is 36-40%, Zr is 0.5-1%, O is 0.8-1.0%, and the balance is Ti.
[0011] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: after the main raw materials for smelting the alloy in the step (1) are proportioned, the TiO2 powder must be grouped according to the specified gram weight of each portion, the grouped TiO2 powder is wrapped with pure titanium foil and shaped into particles, and then the mixture obtained by uniformly mixing sponge titanium and pure niobium particles and the TiO2 particles wrapped with pure titanium foil and shaped are uniformly placed in the crucible of a vacuum melting furnace, and repeatedly smelted in the vacuum melting furnace.
[0012] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein the strategy for evenly placing the mixed material and the TiO2 particles wrapped and shaped by pure titanium foil is as follows: when the total weight of the smelting raw materials is ≤1 kg, the TiO2 particles wrapped and shaped by pure titanium foil are evenly placed in the middle of the mixed material using tweezers; when the total weight of the smelting raw materials is 1 kg < ≤50 kg, first lay a layer of the mixed material with a thickness of 10 to 15 mm and evenly place 4 to 5 TiO2 particles wrapped and shaped by pure titanium foil on it, then lay another layer of the mixed material with a thickness of 10 to 15 mm and evenly place 4 to 5 TiO2 particles wrapped and shaped by pure titanium foil on it, and repeat the above-mentioned even placement strategy in layers; when the total weight of the smelting raw materials is >50 kg, the mixed material and the TiO2 particles wrapped and shaped by pure titanium foil are directly stirred and evenly mixed together.
[0013] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the vacuum melting furnace in the step (1) can use a vacuum magnetic levitation melting furnace, and the raw materials need to be repeatedly melted 3 to 5 times when melting, and the ingots formed after each melting are inverted head to tail between each furnace to ensure the uniformity of the chemical composition of the alloy.
[0014] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the vacuum melting furnace in the step (1) can also use a vacuum non-consumable arc melting furnace, and the raw materials need to be repeatedly melted 6-10 times when melting, and the ingots formed after each melting are inverted upside down between each furnace to ensure the uniformity of the chemical composition of the alloy.
[0015] The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the vacuum melting furnace in the step (1) can also be a vacuum consumable electrode melting furnace.
[0016] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the temperature of the predetermined temperature homogenization heat treatment in the step (2) is 1100-1200°C, and the time is 8-20 h; the temperature of the high temperature forging treatment in the step (2) is 950-1000°C, the insulation time is 5-20 min, and flowing argon gas or high temperature glass protective coating is used for anti-oxidation protection.
[0017] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the high temperature forging treatment in the step (2) is a one-step drawing treatment, and then the high damping titanium alloy profile blank is formed into a plate-shaped high damping titanium alloy profile blank of a predetermined size; the anti-oxidation protection measure in the step (2) can adopt any one of vacuum heat treatment furnace protection, high temperature glass protective coating protection and furnace chamber flowing argon protection; the gradient high temperature annealing process in the step (3) can adopt any one of flowing argon and high temperature glass protective coating for anti-oxidation protection.
[0018] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the temperature of the gradient high temperature annealing treatment adopted in the step (3) is 970-1020°C, the holding time is 20-40min, the alloy is cooled with the furnace to 820-900°C at a predetermined rate of 1-5°C / min, the holding time is 20-120min, and then cooled by water cooling or air cooling with flowing cold air blowing.
[0019] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the multiple-pass rolling process with different reduction amounts in the step (3) can be divided into two stages: in the first stage, when the initial total reduction amount is less than 40-50%, a constant temperature of 550-620°C, a holding time of 3-10 minutes after each pass, and a reduction amount of 0.2-1 mm per pass are used to perform multiple medium-temperature rolling processes; in the second stage, when the total reduction amount is greater than or equal to 40-50%, room temperature rolling is used, and the reduction amount of each pass is 0.2-0.6 mm, until the total reduction amount reaches 85-90%.
[0020] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the multiple-pass rolling process with different reduction amounts in the step (3) can be carried out at a constant temperature of 550-620°C, with a holding time of 5-10 minutes after each pass, a reduction amount of 0.2-1 mm per pass, and multiple-pass medium-temperature rolling treatments are repeated, with a reduction amount of 0.2-0.6 mm per pass, until the total reduction amount reaches 85-90%.
[0021] The preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy, wherein: the annealing temperature of the annealing treatment in the step (4) is 750-920°C, the holding time is 5-30 minutes, and flowing argon is used for anti-oxidation protection during the holding; the cooling treatment in the step (4) is to quickly take the sample out of the furnace and directly throw it into water for cooling.
[0022] By adopting the above technical solution, the present invention has the following beneficial effects:
[0023] The preparation method of the Snoek relaxation type high damping high plasticity titanium alloy of the present invention is reasonable in conception and simple in process. By combining ingot melting, deformation processing and heat treatment process, a high damping high plasticity titanium alloy with a damping coefficient greater than 0.08 and a uniform tensile elongation of more than 20% under room temperature quasi-static conditions is prepared, so as to solve the technical bottleneck problem of brittle fracture of high oxygen content Snoek relaxation type high damping titanium alloy in the elastic stage in the prior art. The present invention can significantly shorten the processing flow and reduce the preparation and processing cost through gradient high temperature treatment and rolling deformation, and greatly improves the production efficiency compared with the traditional method of preparing uniform structure by multi-fire forging and drawing.
[0024] The main features or advantages of the present invention are embodied in the following aspects:
[0025] ① The addition of trace Zr elements has the following main functions: (a) inhibiting the precipitation of hard and brittle ω phase in β phase and improving the work hardening ability of the alloy; (b) as a commonly used grain refiner, significantly refining the alloy ingot structure and improving the processability and deformation ability of the alloy; (c) being beneficial to the stability of α phase and enhancing the controllability of the deformation mode of the remaining β phase in the alloy structure; (d) forming a dense oxide film on the alloy surface under high temperature conditions and improving the oxidation resistance of the alloy surface.
[0026] ② Through gradient high-temperature annealing treatment, the content and spatial distribution of α phase and β phase in the microstructure of high damping titanium alloy can be regulated, which can play the following key roles: (a) Changing the content of α phase can adjust the stability of β phase, thereby obtaining different plastic deformation modes of β phase, such as deformation twinning, stress-induced phase transformation, dislocation slip, etc. Deformation twinning or stress-induced phase transformation will significantly improve the plastic deformation ability of the alloy; (b) Changing the spatial distribution of α phase precipitation, combined with subsequent rolling deformation treatment, can regulate the composition of heterogeneous organization, thereby obtaining the regulation space of mechanical properties and deformation ability; (c) Changing the morphology of α phase precipitation, combined with subsequent rolling deformation treatment, can also regulate the composition of heterogeneous organization;
[0027] ③ The combination of medium temperature and room temperature rolling treatment processes can fully regulate the orientation distribution of the close-packed hexagonal α phase basal plane, cylindrical plane, etc., thereby improving the effect of oxygen elements on the difficulty of slip initiation;
[0028] ④ The annealing process in step (4) can adjust the content of recrystallized lamellae and nanocrystalline matrix structure, thereby obtaining β matrix grains with significant gradient size, significantly improving the plastic deformation ability of the alloy;
[0029] ⑤ The alloy obtained by the preparation method of the present invention has excellent cold / hot processing performance and plastic deformation ability while maintaining good damping performance;
[0030] ⑥ By designing the process parameters of gradient high-temperature annealing, rolling deformation, and annealing, the precipitation of α phase and the stability of β phase were regulated, and heterogeneous structure and deformation twins were obtained. Both of them have the effect of improving the deformation ability of the alloy, thereby significantly improving the plastic deformation ability of the high damping titanium alloy and obtaining a tensile uniform deformation plasticity of more than 20%. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 Schematic diagram of time-temperature of the preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy of the present invention ( Figure 1 In the figure: T0 and t0 represent the temperature and time of homogenization treatment respectively; T1, t1 and ε1 represent the temperature of billet forging, the sample holding time before forging and the deformation of billet forging respectively; t2, t3, t4 represent the time of gradient high temperature treatment respectively; T3 represents the temperature of medium temperature rolling; ε2 and ε3 represent the deformation; T4 is the annealing temperature of the last step);
[0033] Figure 2 The tensile strain-stress relationship curve of the alloy prepared by the preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy of the present invention;
[0034] Figure 3 The graph is a temperature-damping coefficient relationship curve of the alloy prepared by the preparation method of the Snoek relaxation type high-damping high-plasticity titanium alloy of the present invention. DETAILED DESCRIPTION
[0035] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The present invention is further explained below in conjunction with specific implementation modes.
[0037] like Figure 1 As shown, the preparation method of a Snoek relaxation type high damping and high plasticity titanium alloy provided in this embodiment specifically comprises the following steps:
[0038] S001. Using titanium sponge, pure titanium foil, pure niobium particles, pure zirconium flakes and TiO2 powder as the main raw materials for smelting alloy and proportioning them according to a predetermined mass percentage, wherein the TiO2 powder is grouped according to a specified gram weight per portion, and the grouped TiO2 powder is wrapped with pure titanium foil to shape into particles, and the titanium sponge and pure niobium particles are uniformly mixed, and then the mixed material and the TiO2 particles wrapped with pure titanium foil are evenly placed in a crucible, and repeatedly smelted in a vacuum melting furnace and naturally cooled with a water-cooled copper crucible in the furnace to obtain an ingot material of a high damping titanium alloy;
[0039] S002, subjecting the high damping titanium alloy ingot material obtained in the above step S001 to a homogenization treatment within a predetermined temperature-time range and under anti-oxidation protection measures, and then processing it into a plate / rod profile blank through a high temperature forging treatment;
[0040] S003, subjecting the high damping titanium alloy profile blank obtained in the above step S002 to high temperature annealing treatment within a predetermined gradient temperature-time range and under anti-oxidation protection measures, obtaining a primary plate / bar by rolling processing with different reduction amounts for multiple passes, and then subjecting the surface of the rolled primary plate / bar to mechanical grinding and decontamination treatment to obtain a high damping titanium alloy material;
[0041] S004, performing an ordered annealing and cooling treatment on the high damping titanium alloy material obtained in the above step S003 within a predetermined temperature-time range, and finally obtaining a high damping titanium alloy material with a heterogeneous structure.
[0042] Among them, the element mass percentages of the high damping titanium alloy ingot material in the above step S001 are: Nb is 36-40%, Zr is 0.5-1%, O is 0.8-1.0%, and the remainder is Ti.
[0043] The vacuum melting furnace in the above step S001 may be a vacuum magnetic levitation melting furnace, or a vacuum non-consumable arc melting furnace, or a vacuum consumable electrode melting furnace.
[0044] The strategy for evenly placing the mixed material and the capsule in the above step S001 is: when the total weight of the smelting raw materials is less than or equal to 1 kg, use tweezers to evenly place the TiO2 particles wrapped in pure titanium foil and shaped in the middle of the mixed material; when the total weight of the smelting raw materials is greater than 1 kg but ≤50 kg, first lay a layer of 10-15 mm thick mixed material, evenly place 4-5 pure titanium foil wrapped and shaped TiO2 particles on it, and then lay another layer of 10-15 mm thick mixed material, and then evenly place 4-5 pure titanium foil wrapped and shaped TiO2 particles, and repeat this placement strategy in layers; when the total weight of the smelting raw materials is greater than 50 kg, directly stir the mixed material and the pure titanium foil wrapped and shaped TiO2 particles and evenly mix them together.
[0045] When using a vacuum magnetic levitation melting furnace in the above step S001, the melting needs to be repeated 3 to 5 times, and the ingot is turned upside down between each furnace to ensure the uniformity of the chemical composition of the alloy.
[0046] When a vacuum non-consumable arc melting furnace is used in step S001, the melting needs to be repeated 6-10 times, and the ingot is turned upside down between each furnace to ensure the uniformity of the chemical composition of the alloy.
[0047] In the above step S002, the predetermined temperature homogenization heat treatment temperature is 1100-1200° C. and the time is 8-20 h.
[0048] The anti-oxidation protection measures in the above step S002 are to use a vacuum heat treatment furnace, or to use a high-temperature glass protective coating, or to use flowing argon gas protection in the furnace chamber.
[0049] The temperature of the high temperature forging treatment in the above step S002 is 950~1000°C, the insulation time is 5~20 min, and flowing argon gas or high temperature glass protective coating is used for anti-oxidation protection.
[0050] In the above step S002, the high temperature forging process is to perform a secondary drawing process and then shape the blank into a plate / rod profile of a predetermined size.
[0051] The gradient high temperature annealing process used in step S003 is 970-1020°C, the holding time is 20-40min, and the temperature is cooled to 820-900°C with the furnace at a predetermined rate of 1-5°C / min, the holding time is 20-120min, and then cooled by water cooling or air cooling with flowing cold air blowing.
[0052] During the high temperature annealing process in step S003, flowing argon gas or high temperature glass protective coating is used for anti-oxidation protection.
[0053] The multi-pass rolling process used in step S003 can be divided into two stages: in the first stage, when the initial total reduction is less than 40-50%, a constant temperature of 550-620°C is adopted, the holding time after each pass is 3-10 minutes, and the reduction per pass is 0.2-1 mm, and multi-pass medium-temperature rolling treatment is performed; in the second stage, when the total reduction is greater than or equal to 40-50%, room temperature rolling treatment is adopted, and the reduction per pass is 0.2-0.6 mm, until the total reduction reaches 85-90%.
[0054] The multi-pass rolling process used in the above step S003 can be a process of using a constant temperature of 550~620°C, a holding time of 5~10min after each pass, a reduction of 0.2~1mm per pass, and reciprocating multi-pass medium-temperature rolling treatment, with a reduction of 0.2~0.6mm per pass, until the total reduction reaches 85~90%.
[0055] The annealing process used in the above step S004 is an annealing temperature of 750~920°C, a holding time of 5~30min, and the use of flowing argon gas for anti-oxidation protection while keeping warm. The cooling method is to quickly take the sample out of the furnace and throw it directly into water.
[0056] Example 1
[0057] The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy of Example 1 of the present invention, wherein the predetermined weight of the smelting alloy in Example 1 is 200 g, may specifically include the following steps:
[0058] S101. Use sponge titanium, pure titanium foil, pure niobium particles, pure zirconium sheets and TiO2 powder as main raw materials for melting alloy and mix them according to predetermined mass percentages, i.e., the mass percentages of sponge titanium and pure titanium foil are 59.3%, the mass percentage of pure niobium particles is 38%, the mass percentage of pure zirconium sheets is 0.7%, and the mass percentage of TiO2 powder is 2%, wherein the TiO2 powder is divided into 4 groups of 1 gram each, and the grouped TiO2 powder is wrapped with pure titanium foil to be shaped into granules; the sponge titanium and pure niobium particles are uniformly mixed, and then the mixture is put into a crucible of a vacuum non-consumable arc melting furnace, and tweezers are used to evenly place the TiO2 particles wrapped with pure titanium foil in the middle of the mixture; then the vacuum non-consumable arc melting furnace is used for repeated melting for 10 times, and the ingot is inverted between each furnace, and finally the high-damping titanium alloy ingot with uniform composition is obtained by natural cooling with a water-cooled copper crucible in the furnace.
[0059] S102, subjecting the titanium alloy ingot obtained in the above step S101 to homogenization heat treatment in a vacuum heat treatment furnace, specifically at a temperature of 1150° C. and keeping the temperature for 12 h, and then cooling naturally in the vacuum heat treatment furnace.
[0060] S103, the ingot homogenized in the above step S102 is subjected to a high-temperature forging, the sample is placed in a heat treatment furnace with flowing argon protection, the heating temperature is 1000°C and the holding time is 8 minutes, and then the ingot is subjected to a roughening and drawing, the total deformation is more than 200%, and then it is shaped into a 10 mm thick alloy plate billet.
[0061] S104. The plate blank in the above step S103 is subjected to gradient high temperature annealing treatment in a heat treatment furnace protected by flowing argon. The specific implementation process is to keep the sample in a furnace at a temperature of 980°C for 20 min, then cool it to 880°C at a rate of 2°C / min and keep it at that temperature for 40 min, then quickly take the sample out of the furnace and throw it into water for cooling treatment.
[0062] S105. Perform multiple rolling treatments on the samples after the gradient high temperature treatment in the above step S104. The specific implementation is divided into two stages. In the first stage, a constant temperature of 600°C and flowing argon gas are used for protection. The insulation time after each pass is 4 minutes. The reduction per pass is 0.3 mm. Multiple reciprocating medium-temperature rolling treatments are performed. When the initial total reduction is 45%, that is, the sample thickness is rolled to 5.5 mm, the second stage of room temperature rolling treatment is performed. The reduction per pass is 0.2 mm. Multiple reciprocating room temperature rolling is performed until the sample thickness is 1.2 mm, that is, the total reduction reaches 88%. Then, the surface of the plate after cold rolling is mechanically ground and decontaminated.
[0063] S106. The cold-rolled sheet in the above step S105 is annealed under the protection of a flowing argon atmosphere, the annealing temperature is 900°C, the holding time is 10 min, and the cooling method is to quickly take the sample out of the furnace and directly throw it into water, and finally a high-damping and high-plasticity titanium alloy material is obtained.
[0064] Figure 2 The solid line in the middle is the tensile performance curve of the Snoek relaxation type high damping and high plasticity titanium alloy prepared in Example 1. The length of the tensile sample gauge section is 18 mm, the width is 5 mm, and the thickness is 1 mm. The tensile test is carried out using a standard testing machine (Instron 8801) at room temperature, using a 5x10 -4 s -1 The uniaxial tensile test was carried out at a quasi-static tensile rate. The test results show that the yield strength (σ 0.2 ) is 0.96GPa, and the tensile strength (σ b ) is 1.04 GPa and the uniform elongation (ε u ) is 21%, showing excellent strength and plasticity matching and has a wide range of application scenarios.
[0065] Figure 3 The solid line in the middle is the damping coefficient curve of the Snoek relaxation type high damping and high plasticity titanium alloy prepared in Example 1. The damping sample is in the form of a long strip, and the dimensions in the length, width and thickness directions are 56 mm, 1 mm and 6 mm, respectively. The damping test adopts a dynamic thermal mechanical analyzer (DMA, TA Q800), in which the three-point bending mode test is selected. The heating rate is 4°C / min, the frequency is 1Hz, the amplitude is 30μm, and the temperature range is room temperature ±400°C. The test results show that under the preparation conditions of Example 1, the alloy damping coefficient tanδ reaches a peak value of 0.082 at 249°C, which is comparable to the peak value reported.
[0066] It can be seen from this that based on the preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy adopted in Example 1, the high damping titanium alloy can significantly improve the tensile strength and uniform tensile elongation of the alloy while maintaining the original high damping performance, thereby expanding the application range of the alloy.
[0067] Example 2
[0068] The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy of Example 2 of the present invention, wherein the predetermined smelting alloy weight of Example 2 is 10 kg, specifically comprises the following steps:
[0069] S201. Use titanium sponge, pure titanium foil, pure niobium particles, pure zirconium flakes and TiO2 powder as main raw materials for melting alloy and mix them according to predetermined mass percentages, i.e., the mass percentages of titanium sponge and pure titanium foil are 58.2%, the mass percentage of pure niobium particles is 39%, the mass percentage of pure zirconium flakes is 0.8%, and the mass percentage of TiO2 powder is 2%, wherein the TiO2 powder is divided into 40 groups of 1 gram each, and the grouped TiO2 powder is wrapped with pure titanium foil to be shaped into granules; the titanium sponge and pure niobium particles are uniformly mixed, and then the mixture is divided into 9 groups layer by layer and put into a water-cooled copper crucible of a vacuum magnetic levitation melting furnace, and 5 TiO2 particles wrapped with pure titanium foil and shaped are evenly placed in the middle of each layer; then use a vacuum magnetic levitation melting furnace to repeatedly melt for 3 times, and invert the head and tail of the ingot between each furnace to enhance the homogenization of the alloy composition, and finally obtain a high-damping titanium alloy ingot with uniform composition as the water-cooled copper crucible in the melting furnace is naturally cooled.
[0070] S202, subjecting the titanium alloy ingot obtained in the above step S201 to homogenization heat treatment in a vacuum heat treatment furnace, specifically at a temperature of 1200° C. and keeping the temperature for 12 h, and then cooling naturally in the vacuum heat treatment furnace.
[0071] S203, subjecting the ingot homogenized in the above step S202 to a high-temperature forging process, uniformly coating the surface of the sample with high-temperature glass anti-oxidation coating, and then placing the sample in a common heat treatment furnace with a heating temperature of 1000°C and a holding time of 20 minutes, and then subjecting the ingot to a roughening and drawing process with a total deformation of more than 200%, and then shaping it into a 20 mm thick alloy sheet blank.
[0072] S204. The plate blank in the above step S203 is subjected to gradient high temperature annealing treatment in a heat treatment furnace protected by flowing argon gas. The specific implementation process is to keep the sample in a furnace at a temperature of 980°C for 30 min, then cool it to 880°C at a rate of 2°C / min and keep it for 30 min, quickly take the sample out of the furnace and perform water cooling treatment, and then perform surface mechanical grinding and decontamination treatment on the plate after gradient high temperature annealing.
[0073] S205. Perform multiple rolling processes on the sample after the gradient high temperature treatment in the above step S204. Specifically, a constant temperature of 580°C and flowing argon gas are used for protection. The insulation time after each pass is 5 minutes. The reduction amount of each pass is 0.2-0.4 mm. Multiple reciprocating medium-temperature rolling is performed until the sample thickness is 2.2 mm, that is, the total reduction amount reaches 89%. Then, the plate after multiple rolling processes is subjected to surface mechanical grinding and decontamination treatment.
[0074] S206, annealing the rolled plate in the above step S205 under the protection of a flowing argon atmosphere, the annealing temperature is 900°C, the holding time is 10 minutes, and the cooling method is to quickly take the sample out of the furnace and directly throw it into water, and finally obtain a high-damping and high-plasticity titanium alloy material.
[0075] Figure 2 The middle dashed line is the tensile performance curve of the Snoek relaxation type high damping and high plasticity titanium alloy prepared in Example 2. The tensile sample size and experimental test conditions are the same as in Example 1. The test results show that the yield strength (σ 0.2 ) is 0.71GPa, and the tensile strength (σ b ) is 1.0GPa and the uniform elongation (ε u ) is 30%, which also shows excellent strength and plasticity matching.
[0076] Figure 3 The middle dashed line is the damping coefficient curve of the Snoek relaxation type high damping and high plasticity titanium alloy prepared in Example 2. The damping sample size and experimental test conditions are the same as those in Example 1. The test results show that under the preparation conditions of Example 2, the damping coefficient tanδ of the alloy reaches a peak value of 0.091 at 252°C, which is higher than the peak value of the damping coefficient reported previously.
[0077] It can be seen from this that based on the preparation method of the Snoek relaxation type high damping and high plasticity titanium alloy adopted in Example 2, the high damping titanium alloy can significantly improve the tensile strength and uniform tensile elongation of the alloy while maintaining the original high damping performance, thereby expanding the application range of the alloy.
[0078] The present invention utilizes vacuum melting, homogenization treatment, high temperature forging, gradient high temperature precipitation regulation and degradation treatment processes in combination to prepare a high-damping and high-plasticity titanium alloy material with a damping coefficient greater than 0.08, a tensile strength of approximately 1 GPa and a tensile uniform elongation of more than 20%, which is used to solve the technical bottleneck problems of low plasticity and poor processability of Snoek relaxation type high-damping titanium alloy in the prior art.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a Snoek relaxation type high damping and high plasticity titanium alloy, characterized in that: The main steps include: (1) Sponge titanium, pure titanium foil, pure niobium particles, pure zirconium flakes and TiO2 powder are used as raw materials for melting alloys and are proportioned according to a predetermined mass percentage, and then the proportioned raw materials are repeatedly melted in a vacuum melting furnace and naturally cooled in a water-cooled copper crucible in the vacuum melting furnace to obtain a high damping titanium alloy ingot material; (2) subjecting the high damping titanium alloy ingot material obtained in the above step (1) to homogenization treatment at a predetermined homogenization treatment temperature and time range and under anti-oxidation protection measures, and then subjecting the homogenization treatment to high temperature forging treatment to obtain a high damping titanium alloy profile blank; (3) subjecting the high damping titanium alloy profile blank obtained in the above step (2) to a gradient high temperature annealing treatment within a predetermined temperature and time range and under anti-oxidation protection measures, and then subjecting the primary profile blank to a rolling process with multiple passes of different reductions, and then subjecting the surface of the rolled primary profile blank to a mechanical grinding process and a decontamination process to obtain a high damping titanium alloy material; (4) subjecting the high damping titanium alloy material obtained in the above step (3) to an ordered annealing treatment and a cooling treatment within a predetermined temperature and time range, thereby finally obtaining a high damping titanium alloy material with a heterogeneous structure; The element mass percentages of the high damping titanium alloy ingot material in step (1) are: Nb is 36-40%, Zr is 0.5-1%, O is 0.8-1.0%, and the balance is Ti; In the step (3), the gradient high temperature annealing process uses either flowing argon gas or high temperature glass protective coating for anti-oxidation protection; The temperature of the gradient high temperature annealing treatment adopted in the step (3) is 970-1020°C, the holding time is 20-40min, the temperature is cooled to 820-900°C with the furnace at a predetermined rate of 1-5°C / min, the holding time is 20-120min, and then cooled by water cooling or air cooling with flowing cold air blowing; The multi-pass rolling process with different reductions in step (3) is divided into two stages: in the first stage, when the initial total reduction is less than 40-50%, a constant temperature of 550-620°C is adopted, the holding time after each pass is 3-10 minutes, and the reduction of each pass is 0.2-1 mm, and a multi-pass medium-temperature rolling process is performed; In the second stage, when the total reduction is greater than or equal to 40-50%, room temperature rolling is performed, with a reduction of 0.2-0.6 mm per pass, until the total reduction reaches 85-90%; or, the rolling process of multiple passes with different reductions in step (3) is performed at a constant temperature of 550-620°C, with a holding time of 5-10 min after each pass, and a reduction of 0.2-1 mm per pass, and multiple medium temperature rolling processes are repeated, with a reduction of 0.2-0.6 mm per pass, until the total reduction reaches 85-90%; The annealing temperature of the annealing treatment in step (4) is 750-920°C, the insulation time is 5-30 min, and flowing argon gas is used for anti-oxidation protection during insulation; the cooling treatment in step (4) is to quickly take the sample out of the furnace and directly throw it into water for cooling.
2. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 1, characterized in that: After the main raw materials for smelting the alloy in step (1) are proportioned, the TiO2 powder must be grouped according to the specified gram weight of each portion, and the grouped TiO2 powder is wrapped with pure titanium foil to be shaped into particles. Then, the mixture obtained by uniformly mixing the sponge titanium and pure niobium particles and the TiO2 particles wrapped with pure titanium foil are evenly placed in the crucible of a vacuum melting furnace and repeatedly smelted in the vacuum melting furnace.
3. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 2, characterized in that: The strategy for evenly placing the mixed material and the TiO2 particles wrapped and shaped by pure titanium foil is as follows: when the total weight of the smelting raw materials is ≤1 kg, use tweezers to evenly place the TiO2 particles wrapped and shaped by pure titanium foil in the middle of the mixed material; when the total weight of the smelting raw materials is 1 kg < ≤50 kg, first lay a layer of the mixed material 10-15 mm thick and evenly place 4-5 TiO2 particles wrapped and shaped by pure titanium foil on it, then lay another layer of the mixed material 10-15 mm thick and evenly place 4-5 TiO2 particles wrapped and shaped by pure titanium foil on it, and repeat the above-mentioned even placement strategy in this layered manner; when the total weight of the smelting raw materials is >50 kg, directly stir the mixed material and the TiO2 particles wrapped and shaped by pure titanium foil and evenly mix them together.
4. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 1, characterized in that: The vacuum melting furnace in step (1) uses a vacuum magnetic levitation melting furnace. When melting the raw materials, it is necessary to repeatedly melt them 3 to 5 times. Between each melting, the ingots formed after each melting are inverted head to tail to ensure the uniformity of the chemical composition of the alloy.
5. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 1, characterized in that: The vacuum melting furnace in step (1) uses a vacuum non-consumable arc melting furnace. When melting the raw materials, it is necessary to repeatedly melt them 6-10 times. Between each melting, the ingots formed after each melting are inverted upside down to ensure the uniformity of the chemical composition of the alloy.
6. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 1, characterized in that: The vacuum melting furnace in step (1) is a vacuum consumable electrode melting furnace.
7. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 1, characterized in that: The temperature of the predetermined temperature homogenization heat treatment in step (2) is 1100-1200° C. and the time is 8-20 h; In the step (2), the temperature of the high temperature forging treatment is 950-1000° C., the holding time is 5-20 min, and flowing argon gas or high temperature glass protective coating is used for anti-oxidation protection.
8. The method for preparing the Snoek relaxation type high damping and high plasticity titanium alloy according to claim 1, characterized in that: The high temperature forging treatment in step (2) is a one-step drawing treatment, and then the high damping titanium alloy profile blank is formed into a plate-shaped high damping titanium alloy profile blank of a predetermined size; The anti-oxidation protection measure in step (2) is any one of vacuum heat treatment furnace protection, high temperature glass protective coating protection and furnace cavity flowing argon gas protection.
Citation Information
Cited By
Interstitial oxygen-doped multifunctional titanium alloy and preparation method thereof
CN121250183A