Preparation method of low-stress coating for die-casting die
Through high-power pulse magnetron sputtering technology, the Ti transition layer and TiN coating are deposited on the surface of the die-casting mold, and the ratio of metal ions to inert gas ions in the plasma is adjusted, which solves the coating peeling and fracture problems caused by high residual stress, and improves the problem of coating peeling and fracture. Mold life and mechanical properties.
Patent Information
- Application Number
- CN202411090232.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
AI Technical Summary
The die-casting molds have coating peeled off and broken due to high residual stress in high temperature aluminum corrosion and hot and cold alternating environments, resulting in binding failure. The existing low-stress coating preparation methods are complicated or performance losses are lost.
High-power pulse magnetron sputtering technology is used to deposit Ti transition layer and TiN coating on the surface of the die-casting mold substrate in the vacuum chamber. By adjusting the ratio of metal ions to inert gas ions in the plasma, the residual stress of the coating is reduced and the mechanics is improved. performance.
It effectively reduces the residual stress of TiN coating from 6.8GPa to 0.9GPa, improves the hardness, elastic modulus and bonding force of the coating, extends the mold life, and solves the problem of fracture failure caused by high residual stress.
Smart Images

Figure CN119020741A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of low stress coating preparation, and in particular to a method for preparing a low stress coating for a die casting mold. Background Art
[0002] In the harsh service environment of high-temperature aluminum corrosion and hot-cold alternation, the surface of the die-casting mold is often damaged by aluminum corrosion, oxidation, thermal fatigue cracks, etc., and the cyclic thermal stress generated by the hot-cold alternation leads to mold fracture failure. The use of physical vapor deposition (PVD) technology to deposit Ti-based coatings on its surface is currently a relatively effective protective measure. However, the coating often fails to bond due to unstable factors such as peeling or cracking during service. A large number of industrial examples and studies have shown that the high residual stress generated in the coating preparation process is the main reason for its bonding failure.
[0003] At present, there are two main directions for preparing low-stress coatings: one is to release the internal stress of the coating through a combination of soft and hard methods from the perspective of coating structure design, but this method generally requires the coating to have a large thickness and the process flow is relatively complicated; the other is to reduce the ion bombardment energy by reducing the bias voltage from the perspective of coating deposition parameters, thereby reducing the stress of the coating, and its overall performance will inevitably be lost.
[0004] To sum up, it is necessary to make further innovations on existing technologies. Summary of the invention
[0005] In view of the technical problems existing in the above-mentioned background technology, the present invention proposes a method for preparing a low-stress coating for a die-casting mold. The method has a reasonable concept and can effectively improve the life of the die-casting mold, improve the mechanical properties of the coating while reducing the residual stress of the coating, and effectively improve the mold fracture failure caused by the thermal stress generated under the alternation of hot and cold by reducing the coating stress, thereby solving the problem of bonding failure caused by high residual stress on the surface coating of the current die-casting mold.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing a low stress coating for a die casting mold, which mainly comprises the following steps:
[0007] (1) Pre-select the substrate for the die-casting mold and pre-treat it;
[0008] (2) placing the pretreated substrate in a vacuum chamber, introducing high-purity argon gas into the vacuum chamber, cleaning the substrate by high-power pulsed magnetron sputtering, and then cleaning the target material after the high-power pulsed magnetron sputtering;
[0009] (3) In a vacuum chamber, high-power pulsed magnetron sputtering is performed on the surface of the cleaned substrate using a Ti target to deposit a Ti transition layer;
[0010] (4) introducing high-purity nitrogen into the vacuum chamber, and then using a Ti target to perform high-power pulsed magnetron sputtering on the surface of the substrate on which the Ti transition layer has been deposited, so as to deposit a layer of TiN coating;
[0011] (5) The substrate obtained after the deposition of the Ti transition layer and the TiN coating is cooled in a vacuum chamber and then taken out, and finally a low-stress Ti-TiN composite coating is prepared on the surface of the substrate.
[0012] The method for preparing a low-stress coating for a die-casting mold, wherein the process of pre-treating the substrate in step (1) is: first mechanically grinding the substrate, then polishing the ground substrate, then ultrasonically cleaning the polished substrate, and then drying the substrate after ultrasonic cleaning.
[0013] The method for preparing the low stress coating for the die casting mold comprises: the mechanical grinding is performed by using 150# to 2300# water sandpaper; and the polishing is performed by using 0.2μm to 0.4μm diamond polishing paste.
[0014] The method for preparing a low-stress coating for a die-casting mold, wherein the process of ultrasonic cleaning the substrate is: first, the substrate is ultrasonically cleaned in acetone for 10 minutes to 20 minutes to remove dirt, then ultrasonically cleaned in deionized water for 3 minutes to 10 minutes to rinse, and finally ultrasonically cleaned in ethanol for 5 minutes to 15 minutes to dehydrate.
[0015] The method for preparing a low stress coating for a die casting mold, wherein the specific process of step (2) is as follows: first, the vacuum chamber is evacuated to a vacuum degree of 1×10 -3 Pa~5×10 -3 Pa, 160-220sccm high-purity argon is introduced, the main valve angle of the vacuum chamber is adjusted to 30%-50%, so that its working vacuum is 1.0-2PaPa, the DC bias power supply loaded on the substrate is turned on, a bias voltage of -900V--600V is applied to the substrate, and a Ti target is used for sputtering for 10min-30min to clean its surface. During the cleaning, the substrate surface is facing the Ti target; then the bias power supply is turned off, and the DC Ti target power supply is turned on. The DC power supply adopts a constant current mode, and the current parameter of the DC power supply is set to 1A-5A, the argon flow rate is adjusted to 100-250sccm, the main valve angle is adjusted to 60%-90%, so that the working vacuum is 0.4-0.6Pa, and sputtering is performed for 10-15min to achieve target cleaning.
[0016] The method for preparing a low-stress coating for a die-casting mold, wherein the specific process of step (3) is as follows: in a vacuum chamber, the flow rate of argon gas introduced into the vacuum chamber is maintained at 100 to 150 sccm, the main valve angle of the vacuum chamber is set to 60% to 90%, the working vacuum pressure is set to 0.4 to 0.7 Pa, the Ti target is connected to a high-power pulse power supply, and the surface of the substrate is rotated to the opposite side of the Ti target by a rotating device. At this time, the distance between the Ti target and the substrate is set to 70 mm to 100 mm, the power supply parameters of the Ti target are set to a voltage of 600 to 800 V, a pulse width of 60 to 100 μs, and a frequency of 60 to 100 Hz, the bias voltage of the substrate is set to -80 to -200 V, and the surface of the substrate is sputtered for 10 to 30 minutes to deposit a Ti transition layer.
[0017] The method for preparing a low-stress coating for a die-casting mold, wherein the specific process of step (4) is: firstly introducing high-purity nitrogen into the vacuum chamber, and the flow ratio of the introduced nitrogen to argon is in the range of 1:24 to 1:8 sccm; then setting the power supply voltage of the Ti target at 600 to 800 V, the pulse width at 60 to 100 μs, and the frequency at 100 to 550 Hz, so that the average power supply power of the Ti target is 0.4 to 1 kW; setting the substrate bias voltage at -80 V to -120 V; setting the vacuum working pressure of the vacuum chamber at 0.4 to 0.6 Pa; setting the distance between the Ti target and the substrate at 70 to 90 mm; and then using the Ti target to sputter on the substrate surface after the Ti transition layer is deposited for 40 to 60 minutes to deposit a TiN coating.
[0018] The method for preparing a low stress coating for a die casting mold, wherein: in the step (5), the substrate obtained after depositing the Ti transition layer and the TiN coating is cooled in a vacuum chamber for 30 to 60 minutes and then taken out, and finally a low stress Ti-TiN composite coating is prepared on the surface of the substrate.
[0019] The method for preparing a low-stress coating for a die-casting mold comprises: the size of the Ti target used in the high-power pulsed magnetron sputtering is ф72.6×6 mm, and the purity is 99.999%; and the substrate used for the die-casting mold is made of H13 steel.
[0020] The method for preparing a low-stress coating for a die-casting mold, wherein: the high-purity argon gas is argon gas with a gas purity of 99.99%, and the high-purity nitrogen gas is nitrogen gas with a gas purity of 99.99%.
[0021] By adopting the above technical solution, the present invention has the following beneficial effects:
[0022] The preparation method of the low stress coating for the die casting mold of the present invention is reasonably conceived and can effectively improve the service life of the die casting mold. By reducing the stress of the coating, the problem of mold fracture and failure caused by thermal stress generated under hot and cold alternation is effectively improved.
[0023] The present invention uses high-power pulsed magnetron sputtering to prepare a coating on the substrate surface of a die-casting mold. Compared with conventional DC magnetron sputtering, the metal ionization rate of this high-power pulsed magnetron sputtering technology is as high as 70%, which is more conducive to improving the flux ratio of metal ions to inert gas ions. Combined with a plasma full spectrum analyzer and an ion flow acquisition device, the coating can effectively monitor and control the ion flux in the plasma during the deposition process. Based on this, the N Ti+ / N Ar+ The regulation from 2.3 to 7 reduced the residual stress of the TiN coating from 6.8 GPa to 0.9 GPa, and the hardness, elastic modulus and bonding strength of the coating were effectively improved.
[0024] The present invention is combined with the engineering application background, by depositing a Ti-TiN composite coating on a substrate, by regulating the ratio of metal ions to inert gas ions in plasma, and by using metal ion irradiation instead of inert gas ion irradiation, the damage caused by inert gas ion bombardment to the growth of the coating is greatly reduced, and the overall performance of the coating is improved while the residual stress of the coating is effectively reduced. The present invention has no restrictions on the types of metal ions and has a certain universality.
[0025] During the deposition of the coating, high-energy inert gas ions (Ar + ) clamped at lattice defects or gap positions will cause the coating to produce excessive residual compressive stress, while metal ions (film-forming ions) can reduce the growth stress generated during the deposition process because they are mainly bound to the lattice position, and metal ion irradiation also has all the advantages of inert gas ion bombardment. At the same time, the high-energy pulse magnetron sputtering used in the present invention has the characteristics of high ionization rate and ion controllability. Before implementation, the present invention uses metal ion irradiation to replace inert gas ion irradiation from the perspective of reducing coating growth stress by adjusting the ratio of metal ions to inert gas ions in the plasma. While ensuring the advantages of ion irradiation, it also reduces the harm caused by inert gas ion irradiation, and improves the mechanical properties of the coating while reducing the residual stress of the coating, solving the problem of bonding failure caused by high residual stress on the surface coating of the current die-casting mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 A flow chart of a method for preparing a low stress coating for a die casting mold according to the present invention;
[0028] Figure 2 The different metal ions (Ti + ) and inert gas ions (Ar + ) Ion flow variation curve under flux ratio;
[0029] Figure 3 The method for preparing the low stress coating for the die casting mold of the present invention involves different metal ions (Ti + ) and inert gas ions (Ar + )The bonding strength test results of the coating under the flux ratio. DETAILED DESCRIPTION
[0030] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention is further explained below in conjunction with specific implementation modes.
[0032] like Figure 1 As shown, the present embodiment provides a method for preparing a low stress coating for a die casting mold, which specifically includes the following steps:
[0033] S010. Pre-select the substrate for the die-casting mold and pre-treat it. The specific process is: first use 150#~2300# water sandpaper to grind the substrate mechanically, then polish the ground substrate with 0.2μm~0.4μm diamond polishing paste, then ultrasonically clean the polished substrate in acetone for 10min~20min to remove dirt, then ultrasonically clean it in deionized water for 3min~10min, then ultrasonically clean it in ethanol for 5min~15min to dehydrate, and finally dry the substrate.
[0034] S020, place the pretreated substrate in a vacuum chamber, introduce high-purity argon gas into the vacuum chamber, clean the substrate by high-power pulsed magnetron sputtering, and then clean the target material after high-power pulsed magnetron sputtering. The specific process is: first, evacuate the vacuum chamber to a vacuum degree of 1×10 -3 Pa~5×10 -3Pa, 160-220sccm high-purity argon is introduced, the main valve angle of the vacuum chamber is adjusted to 30%-50%, so that its working vacuum is 1.0-2PaPa, the DC bias power supply loaded on the substrate is turned on, a bias voltage of -900V--600V is applied to the substrate, and a Ti target is used for sputtering for 10min-30min to clean its surface. During the cleaning, the substrate surface is facing the Ti target; then the bias power supply is turned off, and the DC Ti target power supply is turned on. The DC power supply adopts a constant current mode, and the current parameter of the DC power supply is set to 1A-5A, the argon flow rate is adjusted to 100-250sccm, the main valve angle is adjusted to 60%-90%, so that the working vacuum is 0.4-0.6Pa, and sputtering is performed for 10-15min to achieve target cleaning.
[0035] S030. In a vacuum chamber, a Ti target is used to perform high-power pulse magnetron sputtering on the surface of the cleaned substrate to deposit a Ti transition layer. The specific process is: in a vacuum chamber, the flow rate of argon gas entering the vacuum chamber is maintained at 100-150 sccm, the main valve angle of the vacuum chamber is set to 60%-90%, the working vacuum pressure is set to 0.4-0.7 Pa, the Ti target is connected to a high-power pulse power supply, and the surface of the substrate is turned to the opposite side of the Ti target through a rotating device. At this time, the distance between the Ti target and the substrate is set to 70mm-100mm, the power supply parameters of the Ti target are set to voltage 600-800V, pulse width 60-100μs, frequency 60-100Hz, and the bias voltage of the substrate is set to -80--200V. The surface of the substrate is sputtered for 10-30min to deposit a Ti transition layer.
[0036] S040, high-purity nitrogen is introduced into the vacuum chamber, and then a Ti target is used to perform high-power pulse magnetron sputtering on the surface of the substrate after the Ti transition layer is deposited to deposit a layer of TiN coating. The specific process is as follows: firstly, high-purity nitrogen is introduced into the vacuum chamber, and the flow ratio of nitrogen to argon is in the range of 1:24 to 1:8sccm; then, the power supply voltage of the Ti target is set at 600 to 800V, the pulse width is set at 60 to 100μs, and the frequency is set at 100 to 550Hz, so that the average power of the Ti target is 0.4 to 1kW; the substrate bias voltage is set at -80V to -120V; the vacuum working pressure of the vacuum chamber is set at 0.4 to 0.6Pa; the distance between the Ti target and the substrate is set at 70 to 90mm; then, the Ti target is used to sputter on the surface of the substrate after the Ti transition layer is deposited for 40 to 60min to deposit the TiN coating.
[0037] S050, cooling the substrate obtained after the Ti transition layer and the TiN coating are deposited in a vacuum chamber for 30 to 60 minutes and then taking it out, and finally preparing a low-stress TiTiN composite coating on the surface of the substrate.
[0038] The high-purity argon gas mentioned above is argon gas with a gas purity of 99.99%, and the high-purity nitrogen gas is nitrogen gas with a gas purity of 99.99%; the size of the Ti target used in high-power pulse magnetron sputtering is ф72.6×6mm, and the purity is 99.999%.
[0039] The present invention utilizes high-power pulsed magnetron sputtering technology and a plasma full spectrum analyzer, and through the regulation of discharge parameters and plasma monitoring, effectively controls the ratio of metal ions to inert gas ions while ensuring a high metal ionization rate; and then adopts a group of experimental parameters with a maximum ratio of metal ions to inert gas ions to prepare a Ti-T i N composite coating, thereby obtaining a TiT i N composite coating with low stress and excellent overall performance.
[0040] Before implementation, the present invention uses a plasma full spectrum analyzer to monitor the plasma, and selects a wavelength of 375.7nm as the wavelength of titanium ions (Ti + ) characteristic spectrum, 364.7nm is the characteristic spectrum of titanium atoms (Ti), 480.0nm is the characteristic spectrum of argon ions (Ar + ) characteristic spectrum. The intensity of each ion is the peak value of the corresponding wavelength in the plasma emission spectrum, using Ti + Strength and Ar + The ratio of the intensity indicates the metal ion (Ti + ) and inert gas ions (Ar + By adjusting the HiPIMS power supply voltage, frequency, pulse width and power parameters, the Ti + With high ionization rate, N Ti+ / N Ar+ The largest set of process parameters, see Figure 2 .
[0041] Example 1
[0042] In Example 1 of the present invention, a titanium target with a size of ф72.6×6 mm and a purity of 99.999% is used, and the gases used are 99.99% high-purity argon and 99.99% high-purity nitrogen. H13 hot-working die steel with a size of 25×25×5 mm is used as the substrate for surface analysis and mechanical property testing of the coating, and the preparation process of the low-stress coating is as follows:
[0043] S110, substrate pretreatment
[0044] H13 steel was mechanically polished with 150#~2300# water-grit sandpaper and polished with 0.2μm diamond polishing paste. It was ultrasonically cleaned in acetone for 15 minutes to remove dirt, ultrasonically cleaned in deionized water for 5 minutes to rinse, and ultrasonically cleaned in ethanol for 10 minutes to dehydrate. It was dried with a hair dryer. Except for grinding and polishing of the silicon wafer, the cleaning process was guaranteed to be consistent with that of H13 steel.
[0045] S120, cleaning target and substrate
[0046] The pretreated substrate was placed in a vacuum chamber and then the vacuum chamber was evacuated to a vacuum degree of 3×10 -3 Pa, introduce 180sccm high-purity argon, adjust the main valve angle of the vacuum chamber to 40% to make its working vacuum 1.0Pa, turn on the DC bias power supply loaded on the substrate, apply a bias of -800V on the substrate, use the Ti target sputtering time for 10min, the purpose is to clean the surface of the substrate and increase its surface activity. At this time, the sample surface is facing the Ti target; then turn off the bias power supply, turn on the DC Ti target power supply, the DC power supply adopts the constant current mode, set the DC power supply current parameter to 2A, adjust the argon flow rate to 120sccm, and adjust the main valve angle to 90%, so that the working vacuum pressure is 0.4Pa, and the sputtering time is 15min. The purpose is to clean the target material and remove impurities and oxide film on the target material surface.
[0047] S130, Ti transition layer deposition
[0048] In the vacuum chamber, the argon flow rate into the vacuum chamber is maintained at 120sccm, the main valve angle is 90%, the working vacuum pressure is 0.4Pa, the Ti target is connected to a high-power pulse magnetron sputtering power supply, and the substrate surface is turned to the opposite side of the target material through a rotating device. At this time, the distance between the Ti target and the substrate is 90mm. When setting the high-power pulse magnetron sputtering, the power supply parameters of the Ti target are voltage 700V, pulse width 100us, frequency 100Hz, and the bias voltage of the substrate is 100V. The surface of the substrate is sputtered for 15min to deposit a Ti transition layer, the purpose of which is to improve the bonding strength between the film and the substrate.
[0049] (4) TiN coating deposition
[0050] First, high-purity nitrogen is introduced into the vacuum chamber, and a Ti N coating is prepared on the substrate by high-power pulsed magnetron sputtering. Specifically, the power supply voltage of the Ti target is 600 V, the pulse width is 80 us, the frequency is 120 Hz, the substrate bias is -80 V, the vacuum working pressure of the vacuum chamber is 0.4 Pa, the average power is 0.6 kW, the flow ratio of nitrogen to argon is 5:120 sccm, the distance between the Ti target and the substrate is 90 mm, and the Ti target is used to sputter on the substrate surface after the Ti transition layer is deposited for 60 minutes to deposit the TiN coating.
[0051] (5) Cooling and removal
[0052] The substrate obtained after the Ti transition layer and the TiN coating are deposited is cooled in a vacuum chamber for 30 minutes and then taken out. The furnace is filled with gas and the H13 steel substrate with the low-stress Ti-TiN composite coating is taken out.
[0053] In this embodiment 1, a Ti transition layer is firstly sputtered on the outer surface of the substrate using high-power pulsed magnetron sputtering technology to improve the bonding force between the film and the substrate. The Ti transition layer has better ductility than the Ti-based ceramic coating. The Ti plasma deposition can promote the bonding between the Ti-based coating and the substrate material. In addition, because the substrate is H13 steel, the thermal expansion coefficients of Fe and Ti are 11.1×10 -6 / K and 10.3×10 -6 / K, the thermal expansion coefficients of the two are close, and the strain inconsistency caused by the different thermal expansion coefficients during the deposition to cooling process is less affected. After the Ti transition layer is deposited, nitrogen is introduced into the vacuum chamber to prepare the TiN coating. Based on this, the N in plasma is first realized. Ti+ / N Ar+ The regulation from 2.3 to 7 reduced the residual stress of the TiN coating from 6.8 GPa to 0.9 GPa, and the hardness, elastic modulus and bonding strength of the coating were effectively improved.
[0054] In Example 1 of the present invention, residual stress, hardness, elastic modulus and bonding strength were tested. The results showed that by increasing the ratio of metal ion irradiation to inert gas ion irradiation and replacing inert gas ion irradiation with metal ion irradiation, the residual stress of the TiN coating can be reduced from 6.8 GPa to 0.9 GPa, and the overall toughness (H / E increased from 0.076 to 0.091) and the film-based bonding performance were improved. The test results are shown in FIG. Figure 3 .
[0055] The present invention has a reasonable concept and can effectively improve the life of the die-casting mold, improve the mechanical properties of the coating while reducing the residual stress of the coating, and effectively improve the mold fracture failure caused by the thermal stress generated under hot and cold alternation by reducing the coating stress, thereby solving the problem of bonding failure caused by high residual stress on the surface coating of the current die-casting mold.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a low stress coating for a die casting mold, characterized in that: The main steps include: (1) Pre-select the substrate for the die-casting mold and pre-treat it; (2) placing the pretreated substrate in a vacuum chamber, introducing high-purity argon gas into the vacuum chamber, cleaning the substrate by high-power pulsed magnetron sputtering, and then cleaning the target material after the high-power pulsed magnetron sputtering; (3) In a vacuum chamber, high-power pulsed magnetron sputtering is performed on the surface of the cleaned substrate using a Ti target to deposit a Ti transition layer; (4) introducing high-purity nitrogen into the vacuum chamber, and then using a Ti target to perform high-power pulsed magnetron sputtering on the surface of the substrate on which the Ti transition layer has been deposited, so as to deposit a layer of TiN coating; (5) The substrate obtained after the deposition of the Ti transition layer and the TiN coating is cooled in a vacuum chamber and then taken out, and finally a low-stress Ti-TiN composite coating is prepared on the surface of the substrate.
2. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: The process of pre-treating the substrate in step (1) is: first mechanically grinding the substrate, then polishing the ground substrate, then ultrasonically cleaning the polished substrate, and then drying the substrate after ultrasonic cleaning.
3. The method for preparing a low stress coating for a die casting mold according to claim 2, characterized in that: The mechanical grinding is performed by using 150#-2300# water sandpaper; the polishing is performed by using 0.2μm-0.4μm diamond polishing paste.
4. The method for preparing a low stress coating for a die casting mold according to claim 2, characterized in that: The process of ultrasonic cleaning the substrate is as follows: firstly, the substrate is ultrasonically cleaned in acetone for 10 to 20 minutes to remove dirt, then ultrasonically cleaned in deionized water for 3 to 10 minutes to rinse, and finally ultrasonically cleaned in ethanol for 5 to 15 minutes to dehydrate.
5. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: The specific process of step (2) is as follows: first, the vacuum chamber is evacuated to a vacuum degree of 1×10 -3 Pa~5×10 -3 Pa, 160-220sccm high-purity argon is introduced, the main valve angle of the vacuum chamber is adjusted to 30%-50%, so that its working vacuum is 1.0-2PaPa, the DC bias power supply loaded on the substrate is turned on, a bias voltage of -900V--600V is applied to the substrate, and a Ti target is used for sputtering for 10min-30min to clean its surface. During the cleaning, the substrate surface is facing the Ti target; then the bias power supply is turned off, and the DC Ti target power supply is turned on. The DC power supply adopts a constant current mode, and the current parameter of the DC power supply is set to 1A-5A, the argon flow rate is adjusted to 100-250sccm, the main valve angle is adjusted to 60%-90%, so that the working vacuum is 0.4-0.6Pa, and sputtering is performed for 10-15min to achieve target cleaning.
6. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: The specific process of step (3) is as follows: in a vacuum chamber, the flow rate of argon gas introduced into the vacuum chamber is maintained at 100-150 sccm, the main valve angle of the vacuum chamber is set to 60%-90%, the working vacuum pressure is set to 0.4-0.7 Pa, the Ti target is connected to a high-power pulse power supply, and the surface of the substrate is rotated to the opposite side of the Ti target by a rotating device. At this time, the distance between the Ti target and the substrate is set to 70mm-100mm, the power supply parameters of the Ti target are set to voltage 600-800V, pulse width 60-100μs, frequency 60-100Hz, the bias voltage of the substrate is set to -80--200V, and the surface of the substrate is sputtered for 10-30min to deposit a Ti transition layer.
7. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: The specific process of step (4) is as follows: firstly, high-purity nitrogen is introduced into the vacuum chamber, and the flow ratio of nitrogen to argon is in the range of 1:24 to 1:8 sccm; then, the power supply voltage of the Ti target is set at 600 to 800 V, the pulse width is set at 60 to 100 μs, and the frequency is set at 100 to 550 Hz, so that the average power supply power of the Ti target is 0.4 to 1 kW; the substrate bias voltage is set at -80 V to -120 V; the vacuum working pressure of the vacuum chamber is set at 0.4 to 0.6 Pa; the distance between the Ti target and the substrate is set at 70 to 90 mm; and then, the Ti target is used to sputter on the substrate surface after the Ti transition layer is deposited for 40 to 60 minutes to deposit a TiN coating.
8. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: In the step (5), the substrate obtained after the Ti transition layer and the TiN coating are deposited is cooled in a vacuum chamber for 30 to 60 minutes and then taken out, and finally a low-stress Ti-TiN composite coating is prepared on the surface of the substrate.
9. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: The size of the Ti target used in the high-power pulse magnetron sputtering is ф72.6×6 mm, and the purity is 99.999%; the substrate used in the die-casting mold is made of H13 steel.
10. The method for preparing a low stress coating for a die casting mold according to claim 1, characterized in that: The high-purity argon gas is argon gas with a gas purity of 99.99%, and the high-purity nitrogen gas is nitrogen gas with a gas purity of 99.99%.