Negative electrode composite material, negative electrode sheet and battery
Through the NiSe2/Ni@C nanoarray material, the problem of poor NiSe2 cycle performance and rate performance was solved. The hydrothermal method was used to synthesize carbon nanosheet arrays modified with heterojunction NiSe2/Ni particles, avoiding polymer binders and Conductive additives improve electrochemical performance and achieve higher cycle stability and rate performance.
Patent Information
- Application Number
- CN202411127586.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-16
AI Technical Summary
NiSe2 has poor circulation and rate performance as a negative electrode material for battery, and its presence in powder form causes polymer binders and conductive additives to be used during electrode preparation, which reduces electrochemical performance.
Using NiSe2/Ni@C nanoarray materials, including carbon cloth substrate, porous carbon nanosheet array and heterojunction NiSe2/Ni particles, the carbon nanosheet array modified by heterojunction NiSe2/Ni particles is synthesized by hydrothermal method to avoid The use of polymer binders and conductive additives improves electrochemical properties.
It alleviates the volume expansion of NiSe2, improves cycling stability and rate performance, optimizes ion diffusion and electron transfer rates, and improves the overall performance of the battery.
Smart Images

Figure CN118676364B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy batteries, and in particular to a negative electrode composite material, a negative electrode sheet and a battery. Background Art
[0002] In recent years, transition metal chalcogenides have attracted much attention as battery negative electrode materials due to their high theoretical capacity and high safety. 2 It shows excellent electrochemical activity. However, due to problems such as low electronic conductivity, volume expansion and electrolyte decomposition, its cycle performance and rate performance are poor. 2 It basically exists in the form of powder. Polymer binders and conductive additives are inevitably used in the electrode preparation process, which not only reduces the contact area and energy density, but also hinders the penetration of electrolyte ions into the electrode, resulting in reduced electrochemical performance.
[0003] Therefore, it is necessary to propose a simple preparation method to solve the problem of NiSe 2 The problem of poor cycle performance and rate performance is solved while solving the existing NiSe 2 Existing in the form of powder, polymer binders and conductive additives are required in the electrode preparation process, resulting in reduced electrochemical performance and complicated preparation process. Summary of the invention
[0004] In view of this, the present invention is committed to providing a negative electrode composite material, a negative electrode plate and a battery to solve the problem of NiSe 2 The problem of poor cycle performance and rate performance is solved while solving the existing NiSe 2 Existing in the form of powder, polymer binders and conductive additives are required in the electrode preparation process, resulting in reduced electrochemical performance and complicated preparation process.
[0005] A first aspect of the present invention provides a negative electrode composite material, the negative electrode composite material comprising NiSe 2 / Ni@C nanoarray material; the NiSe 2 / Ni@C nanoarray materials include:
[0006] (1) Carbon cloth substrate;
[0007] (2) Porous carbon nanosheet arrays;
[0008] (3) Heterojunction NiSe 2 / Ni particles;
[0009] Wherein, the porous carbon nanosheet array is vertically arranged on the surface of the carbon cloth substrate; the heterojunction NiSe 2 / Ni particles are embedded in the porous carbon nanosheet array.
[0010] Optionally, the NiSe 2 / Ni@C nanoarray material has a specific surface area of 300~900m 2 / g.
[0011] Optionally, the sheet diameter of the porous carbon nanosheet array is 1~2μm; and / or, the thickness of the porous carbon nanosheet array is 20~30nm; and / or, the pore diameter of the porous carbon nanosheet array is 10~20nm; and / or, the porosity of the porous carbon nanosheet array is 15~35%.
[0012] Optionally, the heterojunction NiSe 2 / the average particle size of the Ni particles is 30-50 nm; and / or the NiSe 2 The total mass of the NiSe / Ni@C nanoarray material is taken as the reference. 2 / Ni particles content is 60~80wt%.
[0013] A second aspect of the present invention provides a method for preparing a negative electrode composite material, the method comprising the following steps:
[0014] S1, adding a nickel salt, a complexing agent and an organic carbon source into a solvent for mixing to obtain a first material; adding the first material into a reactor with a carbon cloth attached thereto for hydrothermal treatment to obtain a carbon cloth after hydrothermal treatment;
[0015] S2, performing a first washing and a first drying treatment on the carbon cloth after the hydrothermal treatment to obtain a precursor stably grown on the carbon cloth;
[0016] S3, performing selenization treatment on the precursor stably grown on the carbon cloth to obtain a selenized material; performing carbonization treatment on the selenized material to obtain a carbonized material;
[0017] S4, performing a second washing and a second drying process on the carbonized material.
[0018] Optionally, the nickel salt is selected from at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate; and / or the chelating agent is selected from at least one of urea, ammonium fluoride, ethylenediaminetetraacetic acid and hexamethylenetetramine; and / or the organic carbon source is selected from at least one of glucose, sucrose, lactose, fructose, cellulose, starch, organic acid soybean meal, triglycerides, fatty acids, tannic acid, citric acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, asphalt, anthracene and aniline; and / or the solvent is water.
[0019] Optionally, the molar ratio of the nickel salt, the complexing agent and the organic carbon source is 1:3-7:0.1-1.5; and / or the mass ratio of the nickel salt to the solvent is 1:150-250.
[0020] Optionally, in step S1, the mixing treatment is magnetic stirring; the conditions of the magnetic stirring include: stirring time of 20-40 min, stirring speed of 200-400 r / min; and / or, the reactor is a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: temperature of 160-200°C, time of 6-12 h; and / or, in step S2, the washing liquid used in the first washing is selected from anhydrous ethanol and / or water; and / or, the conditions of the first drying treatment include: temperature of 50-70°C, time of 18-36 h; and / or, in step S3, the selenization treatment includes: placing selenium powder upstream of the reactor, placing the precursor stably grown on the carbon cloth under the reactor and / or the carbon cloth is subjected to heat treatment; the mass ratio of the precursor loaded on the carbon cloth to the mass ratio of the selenium powder is 1:2-4; and / or the selenization treatment is carried out in a first protective atmosphere; and / or the selenization treatment temperature is 300-400°C, and the selenization treatment time is 1-2h; and / or the carbonization treatment is carried out in a reducing atmosphere, and the reducing atmosphere comprises hydrogen and a second protective atmosphere; and / or the carbonization treatment conditions comprise: the carbonization temperature is 500-650°C, and the carbonization time is 1-3h; and / or, in step S4, the washing liquid used for the second washing is selected from anhydrous ethanol and / or water; and / or, the second drying treatment conditions comprise: the temperature is 50-70°C, and the time is 18-36h.
[0021] A third aspect of the present invention provides a negative electrode plate, the negative electrode plate comprising a negative electrode material, wherein the negative electrode material comprises the negative electrode composite material mentioned above and / or the negative electrode composite material prepared according to the above method.
[0022] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described above.
[0023] Through the above technical solution, the beneficial technical effects of the present invention are:
[0024] (1) The negative electrode composite material provided by the present invention comprises a heterojunction NiSe 2 NiSe / Ni particle-modified carbon nanosheet array material 2 / Ni@C, the NiSe 2 / Ni@C nanoarray materials include carbon cloth substrate, porous carbon nanosheet array and heterojunction NiSe 2 / Ni particles, this material effectively alleviates the NiSe 2The volume expansion is small, and the ion diffusion and electron transfer rates are excellent, and the cycle stability and rate performance are excellent.
[0025] (2) The preparation method of the negative electrode composite material of the present invention is to synthesize a heterojunction NiSe on a carbon cloth substrate. 2 / Ni particle-modified carbon nanosheet arrays. A carbon source was introduced in situ by a simple one-pot hydrothermal method to prepare a nickel hydroxide composite carbon material nanosheet array precursor, which was then selenized and carbonized to obtain a heterojunction NiSe 2 / Porous carbon nanosheet arrays tightly decorated with Ni particles, namely NiSe grown on carbon cloth 2 / Ni@C nanoarray material. In the carbonization process, the present invention uses a mixed gas with strong reducing properties. When carbonized at high temperature, the organic carbon source has reducing properties in the process of converting to carbon. The carbonization temperature and time are controlled to ensure the success of carbonization. 2 Partially reduced to Ni element to prepare heterojunction NiSe 2 / Ni particles. The heterojunction NiSe 2 / Ni particles reduce the resistance of the negative electrode composite material, the coupled electric field increases the electron transfer rate, enhances the electrochemical kinetics, and improves the rate performance.
[0026] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.
[0028] Figure 1 Shown is an electron microscope scanning image of the negative electrode composite material prepared in Example 1.
[0029] Figure 2 Shown is the X-ray diffraction pattern of the negative electrode composite material prepared in Example 1. DETAILED DESCRIPTION
[0030] The present invention discloses a negative electrode composite material, a negative electrode sheet and a battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0031] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0032] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0033] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0034] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0036] In order to solve the problem of NiSe 2 The problem of poor cycle performance and rate performance is solved while solving the existing NiSe 2 The electrode exists in the form of powder, so polymer binders and conductive additives need to be used in the electrode preparation process, resulting in reduced electrochemical performance and complicated preparation process. The present invention adopts the following technical solution:
[0037] A first aspect of the present invention provides a negative electrode composite material, the negative electrode composite material comprising NiSe 2 / Ni@C nanoarray material; the NiSe 2 / Ni@C nanoarray materials include:
[0038] (1) Carbon cloth substrate;
[0039] (2) Porous carbon nanosheet arrays;
[0040] (3) Heterojunction NiSe 2 / Ni particles;
[0041] Wherein, the porous carbon nanosheet array is vertically arranged on the surface of the carbon cloth substrate; the heterojunction NiSe 2 / Ni particles are embedded in the porous carbon nanosheet array.
[0042] The NiSe contained in the negative electrode composite material of the present invention 2 / Ni@C nanoarray material, the NiSe 2 / Ni@C nanoarray materials include carbon cloth substrate, porous carbon nanosheet array and heterojunction NiSe 2 / Ni particles, this material effectively alleviates the NiSe 2 The volume expansion, cycle stability and rate performance are excellent.
[0043] The porous carbon nanosheet array in the present invention is arranged vertically on the surface of the carbon cloth substrate, which can be specifically manifested as: the porous carbon nanosheet is perpendicular to the surface of the carbon cloth substrate along the extension direction of the sheet diameter, wherein the "vertical" in the present invention means that the extension direction of the sheet diameter of the porous carbon nanosheet is 90º or close to 90º with the plane where the carbon cloth substrate is located.
[0044] The heterojunction NiSe in the present invention 2 / Ni particles are embedded in the porous carbon nanosheet array, which can be specifically manifested as: heterojunction NiSe 2 / Ni particles are only partially embedded in the porous carbon nanosheet array and do not penetrate; and / or, heterojunction NiSe 2 / Ni particles are embedded in and penetrate the porous carbon nanosheet arrays.
[0045] NiSe of the present invention 2 / Ni@C nanoarray material has a large specific surface area to increase the channel for ion migration, shorten the migration path, and improve the rate performance of the battery. 2 / The specific surface area of Ni@C nanoarray materials can be 300~900m 2 / g. For example, the NiSe 2 / Ni@C nanoarray material has a specific surface area of 300m 2 / g, 400 m 2 / g, 500 m 2 / g, 600 m 2 / g, 700 m 2 / g, 800 m 2 / g and 900 m 2 / g or any value within the range of any two of the above values. Preferably, in order to further improve the channel for ion migration, shorten the migration path, and improve the rate performance of the battery, the NiSe 2 / Ni@C nanoarray material has a specific surface area of 500~800m 2 / g.
[0046] In the present invention, suitable diameter and thickness of the porous carbon nanosheets are beneficial to controlling the particle uniformity of the negative electrode composite material.
[0047] According to the present invention, the sheet diameter of the porous carbon nanosheet can be 1-2 μm. Exemplarily, the sheet diameter of the porous carbon nanosheet can be any value among 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm and 2 μm, or any value within the range of any two of the above values. Preferably, the appropriate nanosheet diameter makes the array structure more stable, and the sheet diameter of the porous carbon nanosheet can be 1-1.5 μm.
[0048] According to the present invention, the thickness of the porous carbon nanosheet may be 20-30 nm. Exemplarily, the thickness of the porous carbon nanosheet may be any value among 20 nm, 22 nm, 24 nm, 26 nm, 28 nm and 30 nm or any value within the range of any two of the above values. The thickness of the suitable porous carbon nanosheet can further shorten the ion transmission path while ensuring the structural stability. Preferably, the thickness of the porous carbon nanosheet array may be 20-25 nm.
[0049] According to the present invention, the reasonable pore size distribution of the porous carbon nanosheet array can balance the charge and discharge rate and the cycle life, and improve the overall performance of the battery. The pore size of the porous carbon nanosheet array can be 10-20nm; illustratively, the pore size of the porous carbon nanosheet array can be any value among 10nm, 12nm, 16nm, 18nm and 20nm, or any value within the range of any two of the above values. Preferably, the appropriate pore size can improve the transmission efficiency of ions, and the pore size of the porous carbon nanosheet array can be 15-20nm.
[0050] According to the present invention, the porous carbon nanosheet array has a larger porosity to accommodate more active materials and electrolytes, thereby improving the energy density of the battery. The porosity of the porous carbon nanosheet array can be 15-35%; illustratively, the porosity of the porous carbon nanosheet array can be any value among 15%, 20%, 25%, 30% and 35%, or any value within the range of any two of the above values. Preferably, in order to shorten the transmission path of ions and electrons, the porosity of the porous carbon nanosheet array can be 20-30%.
[0051] According to the present invention, suitable heterojunction NiSe 2 The average particle size of Ni / Ni particles is beneficial to alleviate the 2 The volume expansion of the anode composite material enhances the cycle stability and rate performance of the heterojunction NiSe 2 The average particle size of the Ni / Ni particles can be 30-50 nm; for example, the heterojunction NiSe 2 The average particle size of the Ni / Ni particles can be any value among 30nm, 35nm, 40nm, 45nm and 50nm or any value within the range of any two of the above values. Preferably, the appropriate particle size can ensure the contact area with the electrolyte and the ion transfer speed. 2 The average particle size of the Ni / Ni particles can be 30~40nm.
[0052] According to the present invention, in order to further improve the electrochemical activity of the negative electrode composite material and increase the cycle stability and rate performance of the battery, the present invention contains a large number of heterojunction NiSe 2 / Ni particles. 2 The total mass of the NiSe / Ni@C nanoarray material is taken as the reference. 2 The content of the Ni particles can be 60-80 wt %; for example, the heterojunction NiSe 2 The content of the Ni / Ni particles can be any value among 60 wt%, 65 wt%, 70 wt%, 75 wt% and 80 wt% or any value within the range of any two of the above values. 2 The content of Ni / Ni particles can ensure sufficient capacity and have sufficient carbon material to maintain the stability of the battery cycle structure. 2 The total mass of the NiSe / Ni@C nanoarray material is taken as the reference. 2 / The content of Ni particles is 70~80wt%.
[0053] A second aspect of the present invention provides a method for preparing a negative electrode composite material, the method comprising the following steps:
[0054] S1, adding a nickel salt, a complexing agent and an organic carbon source into a solvent for mixing to obtain a first material; adding the first material into a reactor with a carbon cloth attached thereto for hydrothermal treatment to obtain a carbon cloth after hydrothermal treatment;
[0055] S2, performing a first washing and a first drying treatment on the carbon cloth after the hydrothermal treatment to obtain a precursor stably grown on the carbon cloth;
[0056] S3, performing selenization treatment on the precursor stably grown on the carbon cloth to obtain a selenized material; performing carbonization treatment on the selenized material to obtain a carbonized material;
[0057] S4, performing a second washing and a second drying process on the carbonized material.
[0058] The preparation method of the negative electrode composite material of the present invention is to synthesize a heterojunction NiSe on a carbon cloth substrate 2 / Ni particle modified carbon nanosheet array. The method of the present invention uses a simple one-pot hydrothermal method to hydrolyze the complexing agent to produce hydroxide, and at the same time, nickel ions are combined with it to crystallize and grow on the carbon cloth to form nickel hydroxide. The carbon source is simultaneously compounded with the nickel hydroxide to prepare a carbon cloth with a precursor of a nickel hydroxide composite carbon material nanosheet array; then washing and drying are performed to remove the unstable precursor and impurities attached to the precursor to obtain a precursor stably grown on the carbon cloth; then selenization and carbonization are performed to obtain a heterojunction NiSe 2 / Ni particles tightly modified porous carbon nanosheet array; finally, a second washing and a second drying are performed to remove impurities attached to the array material to obtain NiSe grown on the carbon cloth 2 / Ni@C nanoarray materials.
[0059] According to the present invention, the nickel salt may be selected from at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate.
[0060] According to the present invention, the complexing agent may be selected from at least one of urea, ammonium fluoride, ethylenediaminetetraacetic acid and hexamethylenetetramine.
[0061] In the present invention, an organic carbon source is used as a carbon source. On the one hand, the destruction of the product structure by using an inorganic carbon source can be effectively avoided. On the other hand, the organic carbon source can be reducible at a certain high temperature, which is conducive to the simultaneous reaction of the carbon source with nickel hydroxide. The organic carbon source can be selected from at least one of glucose, sucrose, lactose, fructose, cellulose, starch, organic acid soybean meal, triglyceride, fatty acid, tannic acid, citric acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, asphalt, anthracene and aniline.
[0062] According to the present invention, the solvent may be water.
[0063] According to the present invention, the appropriate amount of carbon source added can improve the cycle life of the material while promoting the hydrothermal nucleation of nickel hydroxide. Optionally, the molar ratio of the nickel salt, the complexing agent and the organic carbon source can be 1:3~7:0.1~1.5, preferably, the molar ratio of the nickel salt, the complexing agent and the organic carbon source can be 1:4~6:0.1~0.5; further preferably, the molar ratio of the nickel salt, the complexing agent and the organic carbon source can be 1:5:0.1~0.5.
[0064] According to the present invention, the mass ratio of the nickel salt to the solvent may be 1:150-250; illustratively, the mass ratio of the nickel salt to the solvent may be any one of 1:150, 1:175, 1:200, 1:225 and 1:250 or any value within the range of any two of the above values. Preferably, the mass ratio of the nickel salt to the solvent may be 1:180-220.
[0065] In an optional embodiment of the present invention, in step S1, the mixing treatment is magnetic stirring; the conditions of the magnetic stirring include: stirring time of 20-40 min, stirring speed of 200-400 r / min. Optionally, the reactor is a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: temperature of 160-200°C, time of 6-12 h; preferably, in order to fully react, the conditions of the hydrothermal treatment include: temperature of 180-200°C, time of 8-12 h.
[0066] In an optional embodiment of the present invention, in step S2, the washing liquid used in the first washing is selected from anhydrous ethanol and / or water. The washing of the present invention can be washing three times with water and ethanol respectively to remove excess growth and unstable impurities. Optionally, the conditions of the first drying treatment include: a temperature of 50-70°C and a time of 18-36 hours.
[0067] In an optional embodiment of the present invention, in step S3, the selenization treatment includes: placing selenium powder upstream of the reactor, placing the precursor stably grown on the carbon cloth downstream of the reactor for heat treatment; the mass ratio of the precursor loaded on the carbon cloth to the mass ratio of the selenium powder is 1:2~4, and the "mass of the precursor loaded on the carbon cloth" in the present invention refers to the weight of the carbon cloth with the precursor stably grown minus the weight of the pure carbon cloth, that is, the precursor loading amount. Optionally, the selenization treatment is carried out in a first protective atmosphere, which can prevent the material from being oxidized by air and cause the product to be impure. Optionally, the selenization treatment temperature is 300~400℃, and the selenization treatment time is 1~2h; and / or, the carbonization treatment is carried out in a reducing atmosphere, which can further ensure the reduction of the nickel element, which is conducive to the crystallization and purity of the product; preferably, the reducing atmosphere includes hydrogen and a second protective atmosphere. In the present invention, the first protective atmosphere and the second protective atmosphere are each independently selected from one of nitrogen, argon, neon, helium, xenon and krypton.
[0068] The carbonization conditions of the present invention may include: a carbonization temperature of 500-650°C and a carbonization time of 1-3 hours; preferably, the carbonization temperature is 550-600°C, and this temperature range can produce uniform amorphous carbon and high temperature is conducive to the formation of NiSe. 2 The present invention uses a mixed gas with strong reducing properties during the carbonization process. When the carbonization is carried out at high temperature, the organic carbon source has reducing properties during the conversion to carbon. The carbonization temperature and time are controlled to ensure the success of the carbonization. 2 Partially reduced to Ni element to prepare heterojunction NiSe 2 / Ni particles.
[0069] In an optional embodiment of the present invention, in step S4, the washing liquid used in the second washing is selected from anhydrous ethanol and / or water. The washing of the present invention can be washing three times with water and ethanol respectively to remove excess growth and unstable impurities. Optionally, the conditions of the second drying treatment include: a temperature of 50-70°C and a time of 18-36 hours.
[0070] A third aspect of the present invention provides a negative electrode plate, the negative electrode plate comprising a negative electrode material, wherein the negative electrode material comprises the negative electrode composite material mentioned above and / or the negative electrode composite material prepared according to the above method.
[0071] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described above.
[0072] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.
[0073] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0074] Example 1
[0075] (1) Weigh 0.04 mol nickel nitrate hexahydrate, 0.2 mol urea, and 0.02 mol lactose into a beaker with a magnetic rod and 2000 mL distilled water, stir for 30 min at a stirring speed of 300 r / min, then add the stirred solution into a polytetrafluoroethylene reactor with a carbon cloth, place the reactor in an oven for hydrothermal reaction, control the hydrothermal temperature at 180 °C, and the hydrothermal time for 8 h.
[0076] (2) The hydrothermal carbon cloth was washed three times with water and ethanol to remove excess growth and unstable impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor stably grown on the carbon cloth.
[0077] (3) Weigh the precursor loading (the precursor loading is equal to the weight of the carbon cloth with the precursor stably grown minus the weight of the pure carbon cloth) and selenium powder in a mass ratio of 1:3, place the magnetic boat containing the selenium powder upstream of the tubular furnace, and place the magnetic boat containing the precursor downstream of the tubular furnace. First, selenization is carried out at a selenization temperature of 400°C, a selenization time of 1.5h, and a first protective atmosphere of nitrogen. After selenization, carbonization is carried out at 500°C for 1h. The reducing atmosphere is hydrogen and the second protective atmosphere is argon. The carbonized material is washed three times with water and ethanol to remove excess impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24h to obtain NiSe grown on carbon cloth. 2 / Ni@C array material.
[0078] (4) Preparation of sodium ion button half-cell: prepared NiSe 2 / Ni@C array negative electrode material as the working electrode, metal sodium sheet as the reference electrode, Whatman GF / D glass fiber as the separator, nickel foam as the spacer and 1 molL − 1 NeA 6 Diethylene glycol methyl ether (Diglyme) solution was used as the electrolyte of the sodium ion battery and a few drops were added. The half-cell was assembled in the order of positive electrode shell, negative electrode material, separator, sodium sheet, nickel foam and negative electrode shell. The assembled half-cell was clamped on the packaging machine with insulating tweezers for sealing. Finally, the packaged battery was taken out of the glove box and left to stand for 24 hours to allow the electrolyte to fully infiltrate before conducting relevant electrochemical tests.
[0079] Example 2
[0080] (1) Weigh 0.04 mol nickel nitrate hexahydrate, 0.2 mol ammonium fluoride, and 0.04 mol cellulose into a beaker with a magnet and 2000 mL distilled water, and stir for 30 min at a stirring speed of 300 r / min. Then add the stirred solution into a polytetrafluoroethylene reactor with a carbon cloth, and place the reactor in an oven for hydrothermal reaction. Control the hydrothermal temperature at 180 °C and the hydrothermal time for 10 h.
[0081] (2) The hydrothermal material was washed three times with water and ethanol to remove excess growth and unstable impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor stably grown on carbon cloth.
[0082] (3) Weigh the precursor loading (the precursor loading is equal to the weight of the carbon cloth with the precursor stably grown minus the weight of the pure carbon cloth) and selenium powder in a mass ratio of 1:3, place the magnetic boat containing the selenium powder upstream of the tubular furnace, and place the magnetic boat containing the precursor downstream of the tubular furnace. First, selenization is carried out at a selenization temperature of 300°C, a selenization time of 2h, and a first protective atmosphere of nitrogen. After selenization, carbonization is carried out at 550°C for 2h. The reducing atmosphere is hydrogen and the second protective atmosphere is argon. The carbonized material is washed three times with water and ethanol to remove excess impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24h to obtain NiSe grown on carbon cloth. 2 / Ni@C array material.
[0083] The method for manufacturing the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0084] Example 3
[0085] (1) Weigh 0.04 mol nickel nitrate hexahydrate, 0.2 mol hexamethylenetetramine, and 0.08 mol tannic acid into a beaker with a magnet and 2000 mL distilled water, and stir for 30 min at a stirring speed of 350 r / min. Then add the stirred solution into a polytetrafluoroethylene reactor with a carbon cloth, and place the reactor in an oven for hydrothermal reaction. Control the hydrothermal temperature at 200 °C and the hydrothermal time for 6 h.
[0086] (2) The hydrothermal material was washed three times with water and ethanol to remove excess growth and unstable impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor stably grown on carbon cloth.
[0087] (3) Weigh the precursor loading (the precursor loading is equal to the weight of the carbon cloth with the precursor stably grown minus the weight of the pure carbon cloth) and selenium powder in a mass ratio of 1:3, place the magnetic boat containing the selenium powder upstream of the tubular furnace, and place the magnetic boat containing the precursor downstream of the tubular furnace. First, selenization is carried out at a selenization temperature of 400°C and a selenization time of 2h. The first protective atmosphere is nitrogen. After selenization, carbonization is carried out at 600°C for 2h. The reducing atmosphere is hydrogen and the second protective atmosphere is argon. The carbonized material is washed three times with water and ethanol to remove excess impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24h to obtain NiSe grown on carbon cloth. 2 / Ni@C array material.
[0088] The method for manufacturing the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0089] Example 4
[0090] (1) Weigh 0.04 mol nickel nitrate hexahydrate, 0.2 mol hexamethylenetetramine, and 0.08 mol tannic acid into a beaker with a magnet and 2000 mL distilled water, and stir for 30 min at a stirring speed of 350 r / min. Then add the stirred solution into a polytetrafluoroethylene reactor with a carbon cloth, and place the reactor in an oven for hydrothermal reaction. Control the hydrothermal temperature at 200 °C and the hydrothermal time for 6 h.
[0091] (2) The hydrothermal material was washed three times with water and ethanol to remove excess growth and unstable impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor stably grown on carbon cloth.
[0092] (3) Weigh the precursor loading (the precursor loading is equal to the weight of the carbon cloth with the precursor stably grown minus the weight of the pure carbon cloth) and selenium powder in a mass ratio of 1:3, place the magnetic boat containing the selenium powder upstream of the tubular furnace, and place the magnetic boat containing the precursor downstream of the tubular furnace. First, selenization is carried out at a selenization temperature of 400°C and a selenization time of 2h. The first protective atmosphere is nitrogen. After selenization, carbonization is carried out at 700°C for 2h. The reducing atmosphere is hydrogen and the second protective atmosphere is argon. The carbonized material is washed three times with water and ethanol to remove excess impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24h to obtain NiSe grown on carbon cloth. 2 / Ni@C array material.
[0093] The method for manufacturing the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0094] Comparative Example 1
[0095] (1) Weigh 0.04 mol of nickel nitrate hexahydrate and 0.2 mol of urea into a beaker with a magnet and 2000 mL of distilled water, stir for 30 min at a speed of 300 r / min, then add the stirred solution into a polytetrafluoroethylene reactor with a carbon cloth, place the reactor in an oven for hydrothermal reaction, control the hydrothermal temperature at 180 °C, and the hydrothermal time for 8 h.
[0096] (2) The hydrothermal material was washed three times with water and ethanol to remove excess growth and unstable impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor stably grown on carbon cloth.
[0097] (3) Weigh the precursor loading (the precursor loading is equal to the weight of the carbon cloth with the precursor stably grown minus the weight of the pure carbon cloth) and selenium powder in a mass ratio of 1:3, place the magnetic boat containing the selenium powder upstream of the tube furnace, and place the magnetic boat containing the precursor downstream of the tube furnace for selenization. The selenization temperature is 300°C, the selenization time is 2h, and the first protective atmosphere is nitrogen. The selenized material is washed three times with water and ethanol to remove excess impurities, and finally dried in a drying oven at a constant temperature of 60°C for 24h to obtain NiSe grown on carbon cloth. 2 Array materials.
[0098] The method for manufacturing the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0099] Comparative Example 2
[0100] (1) Weigh 0.04 mol of nickel nitrate hexahydrate and 0.2 mol of urea into a beaker with a magnet and 2000 mL of distilled water, stir for 30 min, then add the stirred solution into a polytetrafluoroethylene reactor, place the reactor in an oven for hydrothermal reaction, control the hydrothermal temperature at 180 °C, and the hydrothermal time for 8 h.
[0101] (2) The hydrothermal material was washed three times with water and ethanol, and dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0102] (3) Weigh the selenium powder according to the mass ratio of 1:3 for the precursor loading amount and selenium powder, place the magnetic boat with selenium powder upstream of the tube furnace, and place the magnetic boat with the precursor downstream of the tube furnace for selenization. The selenization temperature is 300℃, the selenization time is 2h, and the first protective atmosphere is nitrogen. The selenized material is washed three times with water and ethanol in a high-speed centrifuge, and finally dried in a drying oven at a constant temperature of 60℃ for 24h to obtain NiSe. 2 Powder material.
[0103] (4) Preparation of carbon-free negative electrode sheet: The prepared NiSe 2The powder material, binder (polyvinylidene fluoride (PVDF)), and conductive agent (conductive carbon black (SuperP)) were poured into an agate mortar in a mass ratio of 8:1:1, and mixed and ground for 30 min until the powder was evenly mixed and fine. Then it was poured into a small weighing bottle, and N-methylpyrrolidone solvent was dripped while magnetic stirring until the powder was evenly infiltrated and then the dripping was stopped. Then magnetic stirring was performed for 20 min and ultrasonic treatment was performed for 15 min, and this process was repeated 3 times. The mixed slurry was evenly coated and scraped on the current collector aluminum foil with a coater, and then placed in a drying oven, set to a constant temperature of 80°C, and taken out after drying for 12 h. Then the pole piece was cut into a circular pole piece with a radius of 6 mm with a slicer, and the circular pole piece was compacted with a tablet press and weighed to obtain the negative pole piece.
[0104] The prepared negative electrode was used as the working electrode, the metal sodium sheet was used as the reference electrode, the Whatman GF / D glass fiber was used as the diaphragm, the nickel foam was used as the gasket, and 1 molL −1 NeA 6 Diethylene glycol methyl ether (Diglyme) solution was used as the electrolyte of the sodium ion battery and a few drops were added. The half-cell was assembled in the order of positive electrode shell, negative electrode plate, separator, sodium plate, nickel foam and negative electrode shell. The assembled half-cell was clamped on the packaging machine with insulating tweezers for sealing. Finally, the packaged battery was taken out of the glove box and left to stand for 24 hours to allow the electrolyte to fully infiltrate before conducting relevant electrochemical tests.
[0105] Test Example 1
[0106] 1C / 1C cycle life test: The sodium ion button half-cells prepared in the embodiment and the comparative example were respectively subjected to a 1C / 1C cycle test at 25°C (charge cut-off voltage 3.0V, discharge cut-off voltage 0V).
[0107] The specific measurement method of the discharge capacity after 200 cycles of 1C / 1C is as follows: after the battery has been cycled to 199 cycles, it is charged to 3.0V again and then discharged to 0V at a rate of 0.2C. The discharged capacity divided by the amount of active material is the discharge capacity at the 200th cycle.
[0108] The specific measurement method of the capacity retention rate of 1C / 1C cycle 200 cycles is: 200th cycle discharge specific capacity / first cycle discharge specific capacity.
[0109] The measurement method of the new battery charge transfer resistance and sodium ion diffusion is as follows: the charge transfer resistance of the half-cell is tested using the Autolab electrochemical workstation, and the test frequency is 0.01Hz~100kHz. The obtained data is fitted using the software Z-view to obtain the transfer resistance and sodium ion diffusion coefficient.
[0110] The specific measurement method of the rate discharge ratio of a half-cell is as follows: after the battery is charged to 3.0V, it is discharged to 0V at rates of 0.5C, 1C, 2C, and 5C respectively. The discharged capacity divided by the amount of active material is the discharge specific capacity at different rates.
[0111] Among them, the discharge capacity after 200 cycles of 1C / 1C, the capacity retention rate after 200 cycles of 1C / 1C, the charge transfer resistance of the new battery and the sodium ion diffusion coefficient of the new battery are shown in Table 1. The rate discharge capacity of the half-battery is shown in Table 2.
[0112] The specific measurement method of the rate discharge ratio of a half-cell is as follows: after the battery is charged to 3.0V, it is discharged to 0V at rates of 0.5C, 1C, 2C, and 5C respectively. The discharged capacity divided by the amount of active material is the discharge specific capacity at different rates.
[0113] Table 1
[0114]
[0115] Table 2
[0116]
[0117] It can be seen from the data in Tables 1 and 2 that the negative electrode composite material prepared by the present invention is used for the negative electrode of a sodium ion battery, and the electron transfer rate and ion diffusion rate are significantly improved, and it has lower charging internal resistance and discharge internal resistance, and exhibits better rate performance and cycle performance.
[0118] also, Figure 1 This is a scanning electron microscope image of the negative electrode composite material prepared in Example 1. Figure 1 It can be seen that the negative electrode composite material prepared in Example 1 is an array material. Figure 2 The XRD diagram of the negative electrode composite material prepared in Example 1 is shown in FIG. Figure 2 It can be seen that the negative electrode composite material prepared in Example 1 contains NiSe 2 and Ni.
[0119] Specifically, it can be seen from Table 1 and Table 2 that the negative electrode composite materials prepared in Examples 1 to 5 are applied to sodium ion button half-cells, and the discharge specific capacity at different rates and the discharge specific capacity after 1C / 1C cycles for 200 cycles, the capacity retention rate of 1C / 1C cycles for 200 cycles, and the sodium ion diffusion coefficient of the new battery are significantly improved, and the charge transfer resistance of the new battery is significantly reduced. By comparing Example 3 with Example 4, it can be seen that the carbonization temperature is too high, the discharge specific capacity after 1C / 1C cycles for 200 cycles, the capacity retention rate of 1C / 1C cycles for 200 cycles, and the sodium ion diffusion coefficient of the new battery are reduced, and the discharge specific capacity at different rates is reduced. The negative electrode composite material of Comparative Example 1 was not carbonized during the preparation process, and the NiSe2 Partially reduced to Ni single substance, the discharge specific capacity after 1C / 1C cycle 200 cycles, the capacity retention rate of 1C / 1C cycle 200 cycles and the sodium ion diffusion coefficient of the new battery are significantly reduced, and the discharge specific capacity at different rates is significantly reduced. During the preparation of the negative electrode composite material of Comparative Example 2, no carbon cloth was added to the reactor and no carbonization was performed. In the results, the discharge specific capacity after 1C / 1C cycle 200 cycles, the capacity retention rate of 1C / 1C cycle 200 cycles and the sodium ion diffusion coefficient of the new battery are significantly reduced, and the discharge specific capacity at different rates is significantly reduced.
[0120] Test Example 2
[0121] The negative electrode composite materials prepared in the examples and comparative examples were measured, wherein the specific surface area of the nanoarray material, the pore size of the porous carbon nanosheet array, and the porosity of the porous carbon nanosheet array were measured by nitrogen adsorption and desorption isothermal test. 2 The average particle size of Ni / Ni particles, the diameter of porous carbon nanosheet arrays, and the thickness of porous carbon nanosheet arrays were calibrated by SEM images. 2 The content of Ni / Ni particles was measured by energy dispersive X-ray spectrometer EDS. The test results are shown in Table 3.
[0122] Table 3
[0123]
[0124] It can be seen from the data in Table 3 that the NiSe prepared in Examples 1 to 4 2 / Ni@C nanoarray material has a specific surface area of 500~700m 2 / g, the porous nanosheets have a sheet diameter of 1~1.3μm, a thickness of 20~24nm, a pore size of 15~18nm, and a porosity of 20~28%. Figure 1 It can be seen that the NiSe 2 The porous carbon nanosheet arrays in the Ni@C nanoarray material have rich porous structures and heterojunction NiSe 2 / Ni particles are uniformly embedded in the pores of the porous carbon nanosheet array, and have low charge transfer resistance, high sodium ion diffusion capacity and high electrical performance.
[0125] Compared with Comparative Example 1, the NiSe prepared in Examples 1 to 4 2 Due to the presence of carbon materials, the charge transfer resistance of / Ni@C nanoarray materials is significantly reduced and the sodium ion diffusion coefficient is significantly increased, indicating that the electrochemical reaction kinetics is significantly improved, which is beneficial to the improvement of electrical performance.
[0126] Compared with Examples 1 to 3, the cycle performance and rate performance of Example 4 are significantly reduced, indicating that the carbonization temperature is too high, which has a certain degree of damage to the stability of the material and is not conducive to the electrical performance of the battery.
[0127] Compared with Comparative Example 2, Examples 1 to 4 have a nanoarray structure, which significantly improves the electrochemical reaction kinetics and is beneficial to the performance of battery electrical performance.
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A negative electrode composite material, characterized in that: The negative electrode composite material includes NiSe2 / Ni@C nanoarray material; the NiSe2 / Ni@C nanoarray material includes: (1) Carbon cloth substrate; (2) Porous carbon nanosheet arrays; (3) Heterojunction NiSe2 / Ni particles; Wherein, the porous carbon nanosheet array is vertically arranged on the surface of the carbon cloth substrate; and the heterojunction NiSe2 / Ni particles are embedded in the porous carbon nanosheet array.
2. The negative electrode composite material according to claim 1, characterized in that: The specific surface area of the NiSe2 / Ni@C nanoarray material is 300-900 m 2 / g.
3. The negative electrode composite material according to claim 1, characterized in that: The porous carbon nanosheet array has a sheet diameter of 1-2 μm; And / or, the thickness of the porous carbon nanosheet array is 20-30 nm; And / or, the pore size of the porous carbon nanosheet array is 10-20 nm; And / or, the porosity of the porous carbon nanosheet array is 15-35%.
4. The negative electrode composite material according to claim 1, characterized in that: The average particle size of the heterojunction NiSe2 / Ni particles is 30-50 nm; And / or, based on the total mass of the NiSe2 / Ni@C nanoarray material, the content of the heterojunction NiSe2 / Ni particles is 60-80wt%.
5. A method for preparing the negative electrode composite material according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: S1, adding a nickel salt, a complexing agent and an organic carbon source into a solvent for mixing to obtain a first material; adding the first material into a reactor with a carbon cloth for hydrothermal treatment to obtain a carbon cloth after hydrothermal treatment; S2, performing a first washing and a first drying treatment on the carbon cloth after the hydrothermal treatment to obtain a precursor stably grown on the carbon cloth; S3, performing selenization treatment on the precursor stably grown on the carbon cloth to obtain a selenized material; performing carbonization treatment on the selenized material to obtain a carbonized material; S4, performing a second washing and a second drying process on the carbonized material.
6. The preparation method according to claim 5, characterized in that: The nickel salt is selected from at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate; And / or, the complexing agent is selected from at least one of urea, ammonium fluoride, ethylenediaminetetraacetic acid and hexamethylenetetramine; And / or, the organic carbon source is selected from at least one of glucose, sucrose, lactose, fructose, cellulose, starch, organic acid soybean meal, triglycerides, fatty acids, tannic acid, citric acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, asphalt, anthracene and aniline; And / or, the solvent is water.
7. The preparation method according to claim 5 or 6, characterized in that: The molar ratio of the nickel salt, the complexing agent and the organic carbon source is 1:3-7:0.1-1.5; And / or, the mass ratio of the nickel salt to the solvent is 1:150-250.
8. The preparation method according to claim 5, characterized in that: In step S1, the mixing process is magnetic stirring; the conditions of the magnetic stirring include: stirring time is 20-40 min, stirring speed is 200-400 r / min; And / or, the reactor is a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: a temperature of 160-200° C. and a time of 6-12 h; And / or, in step S2, the washing liquid used in the first washing is selected from anhydrous ethanol and / or water; And / or, the conditions of the first drying treatment include: a temperature of 50-70° C. and a time of 18-36 hours; And / or, in step S3, the selenization treatment includes: placing selenium powder upstream of a reactor, placing the precursor stably grown on the carbon cloth downstream of the reactor for heat treatment; the mass ratio of the precursor loaded on the carbon cloth to the mass ratio of the selenium powder is 1:2-4; and / or, the selenization treatment is performed in a first protective atmosphere; and / or, the selenization treatment temperature is 300-400°C, and the selenization treatment time is 1-2h; And / or, the carbonization treatment is carried out in a reducing atmosphere, the reducing atmosphere includes hydrogen and a second protective atmosphere; and / or, the conditions of the carbonization treatment include: a carbonization temperature of 500-650° C., and a carbonization time of 1-3 hours; And / or, in step S4, the washing liquid used in the second washing is selected from anhydrous ethanol and / or water; And / or, the conditions of the second drying treatment include: a temperature of 50-70° C. and a time of 18-36 hours.
9. A negative electrode plate, characterized in that: The negative electrode plate comprises a negative electrode material, wherein the negative electrode material comprises the negative electrode composite material according to any one of claims 1 to 4 or the negative electrode composite material prepared according to the method according to any one of claims 5 to 8.
10. A battery, characterized in that: The battery comprises the negative electrode sheet according to claim 9.