Composite plastic floor and preparation method thereof

By using fluorocarbon coatings and continuous fiber-reinforced thermoplastic composite PP sheets on composite plastic floors, combined with modified clay, modified lignin and quercetin, traditional composite plastic floors are solved by fading and aging under UV light and high cost of reinforcing materials. The problem of this problem achieves more efficient UV resistance and wear resistance, reduces costs, and improves safety and stability.

CN118683149BActive Publication Date: 2024-11-08ZHEJIANG EXPO NEW MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162525.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
2044-08-23

Smart Images

  • Figure CN118683149B_ABST
    Figure CN118683149B_ABST
Patent Text Reader

Abstract

The present invention is applicable to the technical field of plastic flooring, and provides a composite plastic flooring and a preparation method thereof. The composite plastic flooring comprises an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balancing film in sequence. The coating of the anti-ultraviolet coating comprises a fluorocarbon coating, the wear-resistant layer is a continuous fiber reinforced thermoplastic composite polypropylene (PP) sheet, the base layer adopts PP as a polymer substrate, the balancing film adopts a PP sheet filled with calcium silicate, the balancing film is provided with a coating, the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material and the balancing film material are co-extruded. Compared with the prior art, the present invention not only improves the anti-ultraviolet ability, wear resistance and strength of the composite plastic flooring, but also reduces the cost, improves the safety and stability of use, and has significant advantages and broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plastic floors, and in particular relates to a composite plastic floor and a preparation method thereof. Background Art

[0002] With the development of society and the advancement of science and technology, composite plastic flooring has been widely used in the field of interior decoration due to its advantages such as light weight, durability and easy cleaning. However, during the use of traditional composite plastic flooring, due to exposure to ultraviolet rays, it is easy to fade and age, which affects its service life and appearance. In addition, the wear resistance and strength of composite plastic flooring are also important factors affecting its performance.

[0003] Solutions of the prior art: In order to solve the above problems, the existing solutions are mainly to coat a layer of anti-ultraviolet coating on the surface of the composite plastic floor to improve its anti-ultraviolet ability. At the same time, by adding some reinforcing materials, such as glass fiber, carbon fiber, etc., to improve the wear resistance and strength of the composite plastic floor.

[0004] Problems with existing technologies: First, although the existing anti-ultraviolet coating can improve the anti-ultraviolet ability of composite plastic flooring to a certain extent, its effect is limited and cannot meet the needs of long-term exposure to ultraviolet rays. Secondly, although the existing reinforcing materials can improve the wear resistance and strength of composite plastic flooring, their cost is high and may affect other properties of composite plastic flooring. Therefore, how to improve the anti-ultraviolet ability and reduce the cost while ensuring the performance of composite plastic flooring is a problem that needs to be solved urgently in this field. Summary of the invention

[0005] The present invention provides a composite plastic floor and a preparation method thereof, aiming to solve the above problems.

[0006] The present invention is achieved in this way: a composite plastic floor comprises an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balance film in sequence; the coating of the anti-ultraviolet coating comprises a fluorocarbon coating; the fluorocarbon coating has excellent anti-corrosion performance, extremely low surface energy, excellent hydrophobicity, no dust and scaling, good anti-fouling property, strong adhesion, and ultra-long weather resistance; the coating contains a large number of F--C bonds, which makes it super stable, non-powdering and non-fading; thus, the anti-ultraviolet coating of the present invention has strong anti-ultraviolet ability, can greatly improve the anti-ultraviolet ability of the composite plastic floor, can effectively prevent the composite plastic floor from fading, aging and other problems when exposed to ultraviolet rays for a long time, and improves its service life and aesthetics.

[0007] The wear-resistant layer is a continuous fiber reinforced thermoplastic composite PP sheet, which has good wear resistance and high strength, can effectively improve the wear resistance and strength of the composite plastic floor, and reduces the cost and avoids possible impact on other properties of the composite plastic floor.

[0008] Preferably, the base layer uses polypropylene as a polymer substrate, which has good flame retardant, heat insulation, flame retardant board, moisture-proof and other properties, and can effectively improve the safety and durability of the composite plastic floor; the balancing membrane uses a PP sheet filled with calcium silicate, which has good stability and support, and low cost, and has flame retardant, heat insulation, flame retardant board, moisture-proof and other properties, which improves the safety and stability of the composite plastic floor; the balancing membrane is provided with a coating, and the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material is co-extruded with the balancing membrane material so as to better adhere to the adhesive;

[0009] For example, PP compatibilizer is made by reactive grafting maleic anhydride on polypropylene. Since it introduces a strongly polar side group (maleic anhydride) on the main chain of polypropylene, maleic anhydride grafted polypropylene can become a bridge to enhance the adhesion and compatibility between polar and non-polar materials. Adding PP compatibilizer in the production of filled polypropylene can greatly improve the affinity between filler and polypropylene and the dispersion of filler. This product can be used as a surface improver for extruded plates or sheets, which can effectively improve the surface flatness of sheets or plates and eliminate surface bumps and pitting.

[0010] Maleic anhydride grafted polyolefin has both polar aldehyde groups and olefin non-polar segments, and can achieve a perfect combination of strength and toughness through chemical bonding with polymers and fillers.

[0011] For example, silane grafted polypropylene is an important modified material that can make polypropylene material have better performance. Silane grafted polypropylene is usually used in the preparation of polypropylene composite materials. Its main function is to enhance the mechanical strength, hardness, toughness, wear resistance and corrosion resistance of the composite material.

[0012] The addition of silane grafted polypropylene can improve the mechanical properties of the composite material, making it have higher strength and toughness. Silane grafted polypropylene forms a chemical bond connection inside the material, thereby increasing the wear resistance and corrosion resistance of the material. In addition, silane grafted polypropylene can also improve the processing performance and surface properties of the material, making it easier to process and coat.

[0013] The preparation method of the silane grafted polypropylene composite material is as follows: first, raw materials such as polypropylene, reinforcing material, and silane grafted polypropylene are evenly mixed to form a premix; then the premix is ​​placed in an extruder for extrusion to form a material of a desired shape; finally, the extruded material is heat-treated to form a more solid and durable polymer material.

[0014] Preferably, the coating of the anti-ultraviolet coating further comprises modified clay, modified lignin and quercetin, and the mass ratio of the fluorocarbon coating, modified clay, modified lignin and quercetin is 20-30:2-3:1-2:1.

[0015] Preferably, the preparation method of the modified clay is as follows: 8-12 parts of clay are taken by weight, 30-40 parts of a 10-15% mass fraction of hypochlorous acid aqueous solution are added, heated in a water bath at 30-40°C and stirred for 40-60 minutes, and then a mixture of 0.1-0.3 parts of vinylmethyldimethoxysilane and 2-4 parts of anhydrous ethanol is added, and the temperature is raised to 50-60°C. ℃ and continue stirring for 30-50min, place it in a centrifuge and wash it several times with an organic solvent, and then place it in an oven to dry to obtain modified clay; first, hypochlorous acid is added, heated and stirred, hypochlorous acid is decomposed, oxygen and hydrochloric acid are generated, and hydrochloric acid immersion causes the clay structure to break, showing a porous feature, impurities in the particle channel are dissolved, and the generated oxygen forms small bubbles, enters the interior of the clay, generates pressure, and makes the clay produce a larger space, thereby improving the clay's adsorption and binding ability with other components, and then vinylmethyldimethoxysilane is added to react with the hydroxyl groups on the surface of the clay to form a strong internal chemical structure, improve the mechanical properties of the clay, and by adding modified clay, on the one hand, it can refract light to improve the anti-ultraviolet performance, and on the other hand, it can improve the wear resistance, adhesion, corrosion resistance, weather resistance and other properties of the anti-ultraviolet coating, so that the anti-ultraviolet coating can act for a long time, thereby improving the performance of the composite plastic floor.

[0016] Preferably, the preparation method of the modified lignin is as follows: by weight, lignin and a gluconic acid solution with a concentration of 30-50% are mixed at a solid-liquid ratio of 1:10-20, and the mixture is stirred at 80-100°C for 1-2 hours to obtain modified lignin; the lignin is modified by the gluconic acid solution, and the obtained modified lignin can improve the anti-ultraviolet performance of the anti-ultraviolet coating, and by adding quercetin, the quercetin molecules can be inserted into the lignin macromolecules to form a stable conjugated structure, which protects the antioxidant properties of quercetin and lignin, further improves the antioxidant and anti-aging properties of the anti-ultraviolet coating, and thus improves the performance of the composite plastic floor.

[0017] Preferably, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet include glass fiber mats and / or glass fiber rovings.

[0018] Preferably, the glass fiber mat is a continuous mat, a chopped strand mat or a unidirectional mat, and the PP sheet can be reinforced by combining wollastonite treated with a silane coupling agent and the glass fiber mat.

[0019] Preferably, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet are pretreated by melt impregnation, and the preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: a continuous fiber reinforced polypropylene (PP) unidirectional prepreg tape is obtained by a melt impregnation process, and then its woven fabric is used as a raw material to prepare a continuous fiber reinforced thermoplastic PP composite sheet by a lamination molding method to form a network structure, further improving the wear resistance and strength of the continuous fibers, thereby improving the performance of the composite plastic floor, wherein the mass percentage of the continuous fibers is 10-30%, the preheating temperature is 180-200°C, the molding temperature is 210-230°C, and the molding pressure is 5 MPa.

[0020] Preferably, the continuous fiber reinforced thermoplastic composite PP sheet comprises wollastonite treated with a silane coupling agent and glass fiber mat, the concentration of the silane coupling agent used to treat the wollastonite is 1 wt.%, the mass content of the wollastonite is 20%, and the surface density of the glass fiber mat is 330 g / m 2 The preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: three layers of polypropylene sheets filled with wollastonite treated with a silane coupling agent are stacked and laid with glass fiber felt, and a continuous fiber reinforced PP sheet is obtained after heating, hot pressing, cooling and shaping on a double steel belt continuous melt impregnation equipment.

[0021] The present invention also provides a method for preparing the composite plastic floor, comprising the following steps:

[0022] Prepare various raw materials;

[0023] Making the wear-resistant layer: Cut the continuous fiber reinforced thermoplastic composite PP sheet into the required size. The sheet has a thickness of 1.5 mm and a fiber content of 30-40%. It has good wear resistance and high strength, which can effectively improve the wear resistance and strength of the composite plastic floor and reduce the cost.

[0024] Making an anti-ultraviolet coating: coating an anti-ultraviolet coating on the surface of the wear-resistant layer and drying the coating, wherein the thickness of the anti-ultraviolet coating may be 0.2 mm;

[0025] Making the base layer: Cut the polypropylene substrate into the required size. The thickness of the substrate is 5 mm to ensure that it has excellent flame retardant, heat insulation, moisture-proof and other properties, which improves the safety and stability of the composite plastic floor.

[0026] Making a printing layer;

[0027] Making the balancing membrane: Cut the calcium silicate-filled PP sheet into the required size. The thickness of the sheet is 3 mm to ensure that it has good stability and support, and the cost is low, which can effectively reduce the cost of the composite plastic floor;

[0028] The coating material and the balancing film material are co-extruded to obtain a balancing film with a coating, the thickness of the coating is 0.2 mm, so that the coating and the adhesive have a high degree of adhesion, so that the coating can be better compounded with the base layer, thereby improving the overall performance of the composite plastic floor;

[0029] The wear-resistant layer coated with an anti-ultraviolet coating, the printing layer, the base layer and the balanced film with a coating are stacked in sequence, and then compounded by hot pressing at a temperature of 180°C, a pressure of 10 MPa, and a time of 30 min to obtain a composite plastic floor.

[0030] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0031] 1. The present invention adopts an anti-ultraviolet fluorocarbon coating, which has strong anti-ultraviolet ability and can greatly improve the anti-ultraviolet ability of the composite plastic floor, so that it will not fade, age or other problems even when exposed to ultraviolet rays for a long time, thereby improving its service life and aesthetics.

[0032] 2. The wear-resistant layer of the present invention is a continuous fiber reinforced thermoplastic composite PP sheet. Compared with the glass fiber, carbon fiber and other reinforcing materials in the prior art, it not only improves the wear resistance and strength of the composite plastic floor, but also reduces the cost and avoids the possible impact on other properties of the composite plastic floor.

[0033] 3. The balancing film of the present invention is a PP board filled with calcium silicate, which has the characteristics of flame retardancy, heat insulation, flame retardancy, moisture resistance, etc., and improves the safety and stability of the composite plastic floor.

[0034] 4. The coating material of the present invention is co-extruded with the balancing film material and has a high degree of adhesion with the adhesive, so that it can be better composited with the base layer, thereby improving the overall performance and stability of the composite plastic floor.

[0035] In summary, compared with the prior art, the present invention not only improves the UV resistance, wear resistance and strength of the composite plastic floor, but also reduces the cost, improves the safety and stability of use, and has significant advantages and broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a structural schematic diagram of a composite plastic floor provided by the present invention;

[0037] Figure 2 The present invention provides a flow chart of a method for preparing a composite plastic floor.

[0038] Notes on the accompanying drawings: 1. Anti-UV coating; 2. Wear-resistant layer; 3. Printing layer; 4. Base layer; 5. Balance film. DETAILED DESCRIPTION

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0040] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0041] Example 1

[0042] The embodiment of the present invention provides a composite plastic floor, such as Figure 1 As shown, it includes an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balance film in sequence. The coating of the anti-ultraviolet coating includes a fluorocarbon coating. The fluorocarbon coating has excellent anti-corrosion performance, extremely low surface energy, excellent hydrophobicity, no dust and scaling, good anti-fouling property, strong adhesion, and ultra-long weather resistance. The coating contains a large number of F--C bonds, which makes it super stable and does not powder or fade. Therefore, the anti-ultraviolet coating of the present invention has strong anti-ultraviolet ability, can greatly improve the anti-ultraviolet ability of the composite plastic floor, can effectively prevent the composite plastic floor from fading, aging and other problems when exposed to ultraviolet rays for a long time, and improves its service life and aesthetics.

[0043] The wear-resistant layer is a continuous fiber reinforced thermoplastic composite PP sheet, which has good wear resistance and high strength, and the high strength can effectively improve the wear resistance and strength of the composite plastic floor, and reduce the cost and avoid possible impact on other properties of the composite plastic floor.

[0044] In this embodiment, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet include glass fiber mat and / or glass fiber roving, wherein the glass fiber mat is a continuous mat, a chopped strand mat or a unidirectional mat.

[0045] Furthermore, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet are pretreated by melt impregnation, and the preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: a continuous fiber reinforced polypropylene (PP) unidirectional prepreg tape is obtained by a melt impregnation process, and then its woven fabric is used as a raw material to prepare a continuous fiber reinforced thermoplastic PP composite sheet by a lamination molding method to form a network structure, thereby further improving the wear resistance and strength of the continuous fibers, thereby improving the performance of the composite plastic floor, wherein the mass percentage of the continuous fiber is 10%, the preheating temperature is 180°C, the molding temperature is 210°C, and the molding pressure is 5 MPa.

[0046] The base layer uses polypropylene as a polymer base material, which has good flame retardant and heat insulation, flame retardant board, moisture-proof and other properties, and can effectively improve the safety and durability of the composite plastic floor.

[0047] Specifically, the balancing membrane adopts a PP board filled with calcium silicate, which has good stability and support, low cost, flame retardant and heat insulating, flame retardant board, moisture-proof and other characteristics, thereby improving the safety and stability of the composite plastic floor.

[0048] Preferably, the balancing membrane is provided with a coating, the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material is co-extruded with the balancing membrane material so as to better adhere to the adhesive.

[0049] Example 2

[0050] The embodiment of the present invention provides a composite plastic floor, such as Figure 1 As shown, it includes an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balance film in sequence. The coating of the anti-ultraviolet coating includes a fluorocarbon coating. The fluorocarbon coating has excellent anti-corrosion performance, extremely low surface energy, excellent hydrophobicity, no dust and scaling, good anti-fouling property, strong adhesion, and ultra-long weather resistance. The coating contains a large number of F--C bonds, which makes it super stable and does not powder or fade. Therefore, the anti-ultraviolet coating of the present invention has strong anti-ultraviolet ability, can greatly improve the anti-ultraviolet ability of the composite plastic floor, can effectively prevent the composite plastic floor from fading, aging and other problems when exposed to ultraviolet rays for a long time, and improves its service life and aesthetics.

[0051] The wear-resistant layer is a continuous fiber reinforced thermoplastic composite PP sheet, which has good wear resistance and high strength, and the high strength can effectively improve the wear resistance and strength of the composite plastic floor, and reduce the cost and avoid possible impact on other properties of the composite plastic floor.

[0052] In this embodiment, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet include glass fiber mat and / or glass fiber roving, wherein the glass fiber mat is a continuous mat, a chopped strand mat or a unidirectional mat.

[0053] Furthermore, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet are pretreated by melt impregnation, and the preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: a continuous fiber reinforced polypropylene (PP) unidirectional prepreg tape is obtained by a melt impregnation process, and then its woven fabric is used as a raw material to prepare a continuous fiber reinforced thermoplastic PP composite sheet by a lamination molding method to form a network structure, thereby further improving the wear resistance and strength of the continuous fibers, thereby improving the performance of the composite plastic floor, wherein the mass percentage of the continuous fiber is 20%, the preheating temperature is 190°C, the molding temperature is 220°C, and the molding pressure is 5 MPa.

[0054] The base layer uses polypropylene as a polymer base material, which has good flame retardant and heat insulation, flame retardant board, moisture-proof and other properties, and can effectively improve the safety and durability of the composite plastic floor.

[0055] Specifically, the balancing membrane adopts a PP board filled with calcium silicate, which has good stability and support, low cost, flame retardant and heat insulating, flame retardant board, moisture-proof and other characteristics, thereby improving the safety and stability of the composite plastic floor.

[0056] Preferably, the balancing membrane is provided with a coating, the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material is co-extruded with the balancing membrane material so as to better adhere to the adhesive.

[0057] Example 3

[0058] The embodiment of the present invention provides a composite plastic floor, such as Figure 1 As shown, it includes an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balance film in sequence. The coating of the anti-ultraviolet coating includes a fluorocarbon coating. The fluorocarbon coating has excellent anti-corrosion performance, extremely low surface energy, excellent hydrophobicity, no dust and scaling, good anti-fouling property, strong adhesion, and ultra-long weather resistance. The coating contains a large number of F--C bonds, which makes it super stable and does not powder or fade. Therefore, the anti-ultraviolet coating of the present invention has strong anti-ultraviolet ability, can greatly improve the anti-ultraviolet ability of the composite plastic floor, can effectively prevent the composite plastic floor from fading, aging and other problems when exposed to ultraviolet rays for a long time, and improves its service life and aesthetics.

[0059] The wear-resistant layer is a continuous fiber reinforced thermoplastic composite PP sheet, which has good wear resistance and high strength, and the high strength can effectively improve the wear resistance and strength of the composite plastic floor, and reduce the cost and avoid possible impact on other properties of the composite plastic floor.

[0060] In this embodiment, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet include glass fiber mat and / or glass fiber roving, wherein the glass fiber mat is a continuous mat, a chopped strand mat or a unidirectional mat.

[0061] Furthermore, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet are pretreated by melt impregnation, and the preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: a continuous fiber reinforced polypropylene (PP) unidirectional prepreg tape is obtained by a melt impregnation process, and then its woven fabric is used as a raw material to prepare a continuous fiber reinforced thermoplastic PP composite sheet by a lamination molding method to form a network structure, thereby further improving the wear resistance and strength of the continuous fibers, thereby improving the performance of the composite plastic floor, wherein the mass percentage of the continuous fiber is 30%, the preheating temperature is 200°C, the molding temperature is 230°C, and the molding pressure is 5 MPa.

[0062] The base layer uses polypropylene as a polymer base material, which has good flame retardant and heat insulation, flame retardant board, moisture-proof and other properties, and can effectively improve the safety and durability of the composite plastic floor.

[0063] Specifically, the balancing membrane adopts a PP board filled with calcium silicate, which has good stability and support, low cost, flame retardant and heat insulating, flame retardant board, moisture-proof and other characteristics, thereby improving the safety and stability of the composite plastic floor.

[0064] Preferably, the balancing membrane is provided with a coating, the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material is co-extruded with the balancing membrane material so as to better adhere to the adhesive.

[0065] Example 4

[0066] The embodiment of the present invention provides a composite plastic floor, such as Figure 1As shown, it includes an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balance film in sequence. The coating of the anti-ultraviolet coating includes a fluorocarbon coating. The fluorocarbon coating has excellent anti-corrosion performance, extremely low surface energy, excellent hydrophobicity, no dust and scaling, good anti-fouling property, strong adhesion, and ultra-long weather resistance. The coating contains a large number of F--C bonds, which makes it super stable and does not powder or fade. Therefore, the anti-ultraviolet coating of the present invention has strong anti-ultraviolet ability, can greatly improve the anti-ultraviolet ability of the composite plastic floor, can effectively prevent the composite plastic floor from fading, aging and other problems when exposed to ultraviolet rays for a long time, and improves its service life and aesthetics.

[0067] The wear-resistant layer is a continuous fiber reinforced thermoplastic composite PP sheet, which has good wear resistance and high strength, and the high strength can effectively improve the wear resistance and strength of the composite plastic floor, and reduce the cost and avoid possible impact on other properties of the composite plastic floor.

[0068] In this embodiment, the continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet include glass fiber mat and / or glass fiber roving, wherein the glass fiber mat is a continuous mat, a chopped strand mat or a unidirectional mat.

[0069] Furthermore, the continuous fiber reinforced thermoplastic composite PP sheet comprises wollastonite treated with a silane coupling agent and a glass fiber mat, the concentration of the silane coupling agent for treating the wollastonite is 1 wt.%, the mass content of the wollastonite is 20%, and the surface density of the glass fiber mat is 330 g / m 2 The preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: three layers of polypropylene sheets filled with wollastonite treated with a silane coupling agent are stacked and laid with glass fiber felt, and a continuous fiber reinforced PP sheet is obtained after heating, hot pressing, cooling and shaping on a double steel belt continuous melt impregnation equipment.

[0070] The base layer uses polypropylene as a polymer base material, which has good flame retardant and heat insulation, flame retardant board, moisture-proof and other properties, and can effectively improve the safety and durability of the composite plastic floor.

[0071] Specifically, the balancing membrane adopts a PP board filled with calcium silicate, which has good stability and support, low cost, flame retardant and heat insulating, flame retardant board, moisture-proof and other characteristics, thereby improving the safety and stability of the composite plastic floor.

[0072] Preferably, the balancing membrane is provided with a coating, the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material is co-extruded with the balancing membrane material so as to better adhere to the adhesive.

[0073] Example 5

[0074] In this embodiment, based on the embodiment 2, the coating of the anti-ultraviolet coating further comprises modified clay, modified lignin and quercetin, and the mass ratio of the fluorocarbon coating, the modified clay, the modified lignin and the quercetin is 20:2:1:1.

[0075] The preparation method of the modified clay is as follows: 8 parts of clay are taken by weight, 30 parts of a 10% hypochlorous acid aqueous solution are added, heated in a water bath at 30°C and stirred for 40 minutes, then a mixture of 0.1 parts of vinylmethyldimethoxysilane and 2 parts of anhydrous ethanol is added, the temperature is raised to 50°C and stirring is continued for 30 minutes, the clay is placed in a centrifuge for several times of washing with an organic solvent, and then placed in an oven for drying to obtain the modified clay.

[0076] Specifically, the preparation method of the modified lignin is as follows: by weight, lignin and a 30% gluconic acid solution are mixed at a solid-liquid ratio of 1:10, and stirred at 80° C. for 1 h to obtain modified lignin.

[0077] Example 6

[0078] In this embodiment, based on the embodiment 2, the coating of the anti-ultraviolet coating further comprises modified clay, modified lignin and quercetin, and the mass ratio of the fluorocarbon coating, the modified clay, the modified lignin and the quercetin is 25:2.5:1.5:1.

[0079] The preparation method of the modified clay is as follows: 10 parts of clay are taken by weight, 35 parts of a 13% hypochlorous acid aqueous solution are added, heated in a water bath at 35°C and stirred for 50 minutes, then a mixture of 0.2 parts of vinylmethyldimethoxysilane and 3 parts of anhydrous ethanol is added, the temperature is raised to 55°C, stirring is continued for 40 minutes, the clay is placed in a centrifuge for several times of washing with an organic solvent, and then placed in an oven for drying to obtain the modified clay.

[0080] Specifically, the preparation method of the modified lignin is as follows: by weight, lignin and a 40% gluconic acid solution are mixed at a solid-liquid ratio of 1:15, and stirred at 90° C. for 1.5 h to obtain modified lignin.

[0081] Example 7

[0082] In this embodiment, based on the embodiment 2, the coating of the anti-ultraviolet coating further comprises modified clay, modified lignin and quercetin, and the mass ratio of the fluorocarbon coating, the modified clay, the modified lignin and the quercetin is 30:3:2:1.

[0083] The preparation method of the modified clay is as follows: 12 parts of clay are taken by weight, 40 parts of a 15% hypochlorous acid aqueous solution are added, heated in a water bath at 40°C and stirred for 60 minutes, then a mixture of 0.3 parts of vinylmethyldimethoxysilane and 4 parts of anhydrous ethanol is added, the temperature is raised to 60°C and stirring is continued for 50 minutes, the clay is placed in a centrifuge for several times of washing with an organic solvent, and then placed in an oven for drying to obtain the modified clay.

[0084] Specifically, the preparation method of the modified lignin is as follows: by weight, lignin and a 50% gluconic acid solution are mixed at a solid-liquid ratio of 1:20, and stirred at 100° C. for 2 hours to obtain modified lignin.

[0085] Comparative Example 1: Compared with Example 1, the wear-resistant layer is a common PP sheet.

[0086] Comparative Example 2: Compared with Example 1, no polyolefin mixture coating modified by maleic anhydride or silane grafting is applied on the equilibrium membrane.

[0087] Comparative Example 3: Compared with Example 3, the modified clay was replaced with ordinary clay.

[0088] Comparative Example 4: Compared with Example 3, the modified lignin was replaced by ordinary lignin.

[0089] Comparative Example 5: Compared with Example 3, the invention does not contain quercetin.

[0090] Comparative Example 6: Compared with Example 3, the modified clay was replaced by common clay, the modified lignin was replaced by common lignin, and quercetin was not included.

[0091] Comparative Example 7: A commercially available composite plastic floor.

[0092] Experiment 1

[0093] Wear resistance: The wear resistance of the composite plastic floors of Examples 1-4, Comparative Example 1 and Comparative Example 7 was tested with reference to GBT18102-2007 standard. The results are shown in Table 1:

[0094]

[0095] It can be seen from the above results that the composite plastic floor prepared by the present invention has good wear resistance.

[0096] Experiment 2

[0097] The composite plastic floors of Examples 1-4 and Comparative Examples 1, 2 and 7 were subjected to mechanical property tests and impact property tests. The mechanical property test was conducted using an electronic universal material testing machine; the impact property test was conducted using an impact property tester. The test results are shown in Table 2 below:

[0098]

[0099] It can be seen from the above results that the composite plastic floor prepared by the present invention has good impact resistance and mechanical properties.

[0100] Experiment 3

[0101] The performance of the floorings of Examples 1-7 and Comparative Examples 3-7 was tested according to the test method of the international standard ISO11507:1997 "Paints and varnishes - Artificial weathering of coatings - Exposure to fluorescent ultraviolet light and water". The floorings of Examples 1-7 and Comparative Examples 3-7 were cut into samples with a specification of 95 mm × 45 mm, respectively. The samples were continuously illuminated under UVA (340) lamps for 180 hours. The color change (△E*) results are shown in Table 3:

[0102]

[0103] From the above results, it can be seen that the composite plastic floor of the present invention has good anti-ultraviolet performance, especially by adding modified clay, modified lignin and quercetin, the three have a synergistic effect and can further improve the anti-ultraviolet performance of the anti-ultraviolet coating.

[0104] It should be noted that, for the above embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.

[0105] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. A composite plastic floor, It is characterized in that It includes an anti-ultraviolet coating, a wear-resistant layer, a printing layer, a base layer and a balance film in sequence, wherein the coating of the anti-ultraviolet coating includes a fluorocarbon coating, and the wear-resistant layer is a continuous fiber reinforced thermoplastic composite PP sheet; The base layer uses polypropylene as a polymer substrate; the balancing membrane uses a PP sheet filled with calcium silicate, and the balancing membrane is provided with a coating, the coating material is maleic anhydride or silane grafted modified polypropylene, and the coating material is co-extruded with the balancing membrane material; The coating of the anti-ultraviolet coating also includes modified clay, modified lignin and quercetin, and the mass ratio of the fluorocarbon coating, the modified clay, the modified lignin and the quercetin is 20-30:2-3:1-2:1; The preparation method of the modified clay is as follows: 8-12 parts of clay are taken by weight, 30-40 parts of a hypochlorous acid aqueous solution with a mass fraction of 10-15% are added, the mixture is heated in a water bath at 30-40°C and fully stirred for 40-60 minutes, then 0.1-0.3 parts of a mixture of vinylmethyldimethoxysilane and 2-4 parts of anhydrous ethanol are added, the temperature is raised to 50-60°C and stirring is continued for 30-50 minutes, the clay is placed in a centrifuge for several times of washing with an organic solvent, and then placed in an oven for drying to obtain the modified clay; The preparation method of the modified lignin is as follows: by weight, lignin and a gluconic acid solution with a concentration of 30-50% are mixed at a solid-liquid ratio of 1:10-20, and stirred at 80-100° C. for 1-2 h to obtain the modified lignin; The continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet include glass fiber mat and / or glass fiber roving.

2. The composite plastic floor as claimed in claim 1, It is characterized in that The glass fiber mat is a continuous mat, a chopped strand mat or a unidirectional mat.

3. The composite plastic floor as claimed in claim 1, It is characterized in that The continuous fibers used in the continuous fiber reinforced thermoplastic composite PP sheet are pretreated by melt impregnation. The preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: a continuous fiber reinforced polypropylene unidirectional prepreg tape is obtained by a melt impregnation process, and then its woven fabric is used as a raw material to prepare a continuous fiber reinforced thermoplastic PP composite sheet by a lamination molding method, the mass percentage of the continuous fiber is 10-30%, the preheating temperature is 180-200°C, the molding temperature is 210-230°C, and the molding pressure is 5 MPa.

4. The composite plastic floor as claimed in claim 1, It is characterized in that The continuous fiber reinforced thermoplastic composite PP sheet comprises wollastonite treated with a silane coupling agent and a glass fiber mat, wherein the concentration of the silane coupling agent used to treat the wollastonite is 1wt.%, the mass content of the wollastonite is 20%, and the surface density of the glass fiber mat is 330 g / m 2 The preparation method of the continuous fiber reinforced thermoplastic composite PP sheet is as follows: three layers of polypropylene sheets filled with wollastonite treated with a silane coupling agent are stacked and laid with glass fiber felt, and a continuous fiber reinforced PP sheet is obtained after heating, hot pressing, cooling and shaping on a double steel belt continuous melt impregnation equipment.

5. A method for preparing a composite plastic floor according to any one of claims 1 to 4, It is characterized in that The steps include: Prepare various raw materials; Making wear-resistant layer; Make UV-resistant coatings; Making the grass roots; Making a printing layer; Co-extruding the coating material and the balancing film material to obtain a balancing film with a coating; The wear-resistant layer coated with an anti-ultraviolet coating, the printing layer, the base layer and the balancing film with a coating are stacked in sequence, and then compounded by hot pressing at a temperature of 180°C to obtain a composite plastic floor.