Carbon nitride nanospheres, preparation method, application and composite material thereof
Carbon nitride nano microspheres were prepared by ball milling, and the polymerization process was controlled by microcrystals and grinders, which solved the problems of low catalytic activity and poor circulation performance of existing carbon nitride materials, and achieved high catalytic activity and good circulation performance of nitrogen Carbonized nanomicrospheres have enhanced their application potential in the field of photocatalysis.
Patent Information
- Application Number
- CN202411162382.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing carbon nitride materials have low catalytic activity and poor circulation performance, making it difficult to show excellent catalytic performance in the field of photocatalysis.
By ball milling the carbon nitride precursor and microcrystals, carbon nitride nano microspheres are formed, and the polymerization process is controlled by the microcrystals and the grinding body provides local high temperatures, and carbon nitride nano micro micrometers with high catalytic activity and good cycle performance are prepared. ball.
The high catalytic activity and good cycling performance of carbon nitride nano microspheres have been achieved, which has improved its application potential in the field of photocatalytic, especially in the fields of photocatalytic degradation and energy catalysis.
Smart Images

Figure CN118684201B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic materials, and in particular relates to carbon nitride nano-microspheres, a preparation method, an application and a composite material thereof. Background Art
[0002] In recent years, photocatalytic technology that uses semiconductor materials with light response ability to drive the conversion of solar energy and convert light energy into chemical energy has received widespread attention in various fields of energy shortage and environmental governance. Among them, the characteristics of semiconductor materials such as light response and absorption ability, specific surface area, charge transfer ability, conduction band valence band position, and active sites directly determine the photocatalytic performance of semiconductor materials. Carbon nitride was first reported by Professor Wang Xinchen in 2009. It has a two-dimensional planar structure similar to graphene, visible light response ability, and suitable energy band structure, etc., and exhibits excellent photocatalytic hydrogen production performance. However, since carbon nitride is synthesized by high-temperature calcination of nitrogen-containing precursors, that is, the traditional solid-phase method, which leads to strong interaction between its layers, the carbon nitride synthesized by the solid-phase method exhibits a very small specific surface area. This is not conducive to the catalyst's response and absorption ability to light, nor is it conducive to the transfer of charge on the catalyst surface. Moreover, in the field of photocatalytic synthesis, conversion, and degradation, a small specific surface area will lead to a reduction in the contact area between the catalyst and the reactant, which is not conducive to the photocatalytic reaction.
[0003] In order to improve the catalytic activity of carbon nitride materials, designing and synthesizing carbon nitride materials with special morphology, increasing their specific surface area, and making them exhibit excellent catalytic activity has become a hot topic for researchers. This strategy is mainly divided into two modes: top-down and bottom-up, that is, post-processing the synthesized carbon nitride and modifying the carbon nitride precursor. The corresponding specific operation methods include hard template method, soft template method, supramolecular method, protonation method, concentrated acid intercalation, etc. Feng et al. synthesized carbon nitride materials with rod-like structures by using the improved Hummers method. The carbon nitride materials were first synthesized and the initial carbon nitride was treated with strong acid and strong oxidant (Journal of Colloid Interface Science, 2016, 479: 1-6). Tang et al. mixed urea with melamine, generated a supramolecular precursor with a tubular structure by preheating, and then calcined it to prepare carbon nitride nanotubes with a porous structure (Small, 2023, 19: 2208232). It can be seen that both the post-treatment process and the pre-treatment process can improve the layer stacking phenomenon of carbon nitride and obtain carbon nitride materials with special morphology. In addition, Jiang et al. used a ball milling process to prepare a hexagonal boron nitride catalyst with modified -OH and -NH groups on the edge, and obtained a high NO conversion rate of 97.94% and a N selectivity of 97.31% in the absence of additional hole scavengers (Chemical Engineering Journal, 2022, 428(15): 131054). However, the current synthesis and improvement methods still cannot obtain a carbon nitride material with high catalytic activity and good cycle performance. Summary of the invention
[0004] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to overcome the problems of low catalytic activity and poor cycle performance of existing carbon nitride materials, and to propose a carbon nitride nano-microsphere with high catalytic activity and good cycle performance, and a preparation method, application and composite material thereof.
[0005] In order to solve the technical problem, the technical solution adopted by the present invention is:
[0006] On one hand, the present invention provides a method for preparing carbon nitride nano-microspheres, comprising: fully mixing a carbon nitride precursor, adding microcrystals, and then ball-milling with a grinding body to obtain carbon nitride nano-microspheres; the carbon nitride precursor is a nitrogen-rich organic compound; the microcrystals are selected from one of halide salts, KSCN, or Na2SO4; the radius of the grinding body is 1-3 mm; or the radius of the grinding body is 5-10 mm; or the grinding body is composed of a grinding body with a radius of 1-3 mm and a grinding body with a radius of 5-10 mm; the ball milling speed is selected from any value in the range of 200-500 r / min, and the ball milling time is selected from any value in the range of 1-6 h.
[0007] Preferably, the nitrogen-rich organic compound is selected from one or more of urea, cyanamide, dicyandiamide, melamine, thiourea, and dimethylformamide; the microcrystals are selected from one of halide salts, KSCN, or Na2SO4; and the grinding body is a pickaxe ball.
[0008] Preferably, the nitrogen-rich organic compound is selected from melamine and urea, and the mixing mass ratio of the melamine to the urea is 1:1-1:20.
[0009] Preferably, the mass ratio of the microcrystals to the carbon nitride precursor is 5:1-1:5; the mass ratio of the carbon nitride precursor to the grinding body is 1:30-1:100.
[0010] Preferably, the fully mixing of the carbon nitride precursor comprises: firstly mixing by at least one of hydrothermal, stirring or shaking, and then drying by at least one of vacuum oven drying, heating evaporation drying, rotary evaporation drying or freeze drying.
[0011] Preferably, the ball milling mode includes revolution, rotation, or a combination of revolution and rotation.
[0012] Preferably, the method further comprises: calcining the sample obtained after ball milling by a solid phase method, grinding, washing with water and then drying to obtain the carbon nitride nanospheres; the atmosphere used in the solid phase method comprises an inert gas or static air, and the gas flow rate of the inert gas is 20-100 mL / min; the calcination temperature is 400-800°C; the calcination procedure comprises heating to the target temperature in one step or heating to the target temperature in steps; the heating rate of the calcination is 0.1-10°C / min; and the calcination time is 1-6 h.
[0013] The present invention also provides a carbon nitride nano-microsphere, which is prepared by the preparation method of the carbon nitride nano-microsphere described in any one of the above technical solutions.
[0014] Another aspect of the present invention provides the use of the carbon nitride nano-microspheres in the fields of catalytic degradation and energy catalysis.
[0015] The present invention also provides a composite material, comprising the carbon nitride nano-microspheres described in any one of the above technical solutions.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention provides a method for preparing carbon nitride nano-microspheres, wherein grinding causes a precursor to generate a local high temperature, so that the precursor is pretreated and micro-polymerized to form a supramolecular precursor. In this process, the presence of microcrystals will occupy the polymerization position, limit the degree of polymerization of the precursor at the local high temperature, and controllably form a micro-supramolecular precursor. The presence of microcrystals can also enhance the mechanical grinding strength, assist the local high temperature, and act as a control agent for the pretreatment micro-polymerization process during the thermal polymerization of the micro-supramolecular precursor to limit the growth of carbon nitride crystals, control the polymerization of the supramolecular precursor and limit the growth of the carbon nitride crystals, and finally form carbon nitride nano-microspheres with a limited appearance.
[0018] The invention also provides a carbon nitride nano-microsphere, which has the characteristics of high catalytic activity and good cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope image of the carbon nitride material prepared in Example 1 of the present invention;
[0020] Figure 2 This is a scanning electron microscope image of the carbon nitride material prepared in Example 2 of the present invention;
[0021] Figure 3 This is a scanning electron microscope image of the carbon nitride material prepared in Example 3 of the present invention;
[0022] Figure 4 This is a scanning electron microscope image of the carbon nitride material prepared in Comparative Example 1 of the present invention;
[0023] Figure 5 This is a scanning electron microscope image of the carbon nitride material prepared in Comparative Example 2 of the present invention;
[0024] Figure 6 This is a scanning electron microscope image of the carbon nitride material prepared in Comparative Example 3 of the present invention;
[0025] Figure 7 This is an X-ray diffraction pattern of the carbon nitride material prepared in Example 1 of the present invention;
[0026] Figure 8 The electron paramagnetic resonance spectra of the carbon nitride materials prepared in Example 1 and Comparative Example 3 of the present invention;
[0027] Fig. 9 This is a comparison chart of the degradation performance of carbon nitride materials prepared in Example 1 and Comparative Example 3 of the present invention;
[0028] Fig.10 This is a cyclic stability performance diagram of Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The technical scheme in the specific embodiment of the present invention is described in detail and completely below. Obviously, the described embodiment is only a part of the specific implementation of the overall technical scheme of the present invention, rather than all implementations. Based on the overall concept of the present invention, all other embodiments obtained by ordinary technicians in this field fall within the scope of protection of the present invention.
[0030] On one hand, the present invention provides a method for preparing carbon nitride nano-microspheres, comprising: fully mixing a carbon nitride precursor, adding microcrystals, and then ball-milling with a grinding body to obtain carbon nitride nano-microspheres; the carbon nitride precursor is a nitrogen-rich organic compound; the microcrystals are selected from one of halide salts, KSCN, or Na2SO4; the radius of the grinding body is 1-3 mm; or the radius of the grinding body is 5-10 mm; or the grinding body is composed of a grinding body with a radius of 1-3 mm and a grinding body with a radius of 5-10 mm; the ball milling speed is selected from any value in the range of 200-500 r / min, and the ball milling time is selected from any value in the range of 1-6 h.
[0031] Strong mechanical grinding will cause the precursor to generate local high temperature, so that the precursor is pretreated and micro-polymerized to form a supramolecular precursor. In this process, the presence of microcrystals will occupy the polymerization position, limit the degree of polymerization of the precursor at local high temperature, and controllably form a tiny supramolecular precursor. The presence of microcrystals can also enhance the mechanical grinding strength, and limit the growth of carbon nitride crystals during the thermal polymerization of the tiny supramolecular precursor, and finally form carbon nitride nano-microspheres. During the operation of the above-mentioned preparation method, a ball mill is used to provide strong mechanical grinding for the precursor, so that the precursor generates local high temperature. Microcrystals can enhance the grinding force, assist local high temperature, and can be used as a control agent for the pretreatment micro-polymerization process to control the polymerization of supramolecular precursors and limit the growth of carbon nitride crystals.
[0032] The above preparation method specifically defines the use of a ball mill to provide strong mechanical grinding for the precursor, and further defines the radius of the grinding body, the ball milling speed and the ball milling time, which is conducive to controlling the temperature of the local high temperature generated by grinding, and effectively controlling the polymerization process to proceed stably in the set direction. It is understood that the radius of the grinding body can also be 2 mm, 6 mm, 7 mm, 8 mm, or 9 mm; the ball milling speed can also be 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min and any point value within the range; the ball milling time can also be 2 h, 3 h, 4 h, 5 h and any point value within the range.
[0033] The above technical solution further limits the microcrystals to be selected from one of halide salts, KSCN, or Na2SO4. The reason is that the above types of microcrystals can not only enhance the grinding force and assist local high temperature, but also serve as a controller for the pretreatment micropolymerization process, control the polymerization of supramolecular precursors and limit the growth of carbon nitride crystals.
[0034] In a preferred embodiment, the nitrogen-rich organic compound is selected from one or more of urea, cyanamide, dicyandiamide, melamine, thiourea, and dimethylformamide; the microcrystals are selected from one of halide salts, KSCN, or Na2SO4; and the grinding body is a pickaxe ball.
[0035] In a preferred embodiment, the nitrogen-rich organic compound is selected from melamine and urea, and the mixing mass ratio of the melamine and the urea is 1:1-1:20. It is understandable that the mixing mass ratio of melamine and urea can also be 1:5, 1:10, 1:15 and any point value ratio within the range.
[0036] In a preferred embodiment, the mass ratio of the microcrystals to the carbon nitride precursor is 5:1-1:5; the mass ratio of the carbon nitride precursor to the abrasive body is 1:30-1:100. It is understood that the mass ratio of the carbon nitride precursor to the abrasive body can also be 1:40, 1:50, 1:60, 1:70, 1:80, 1:90 and any point value within the range thereof.
[0037] In a preferred embodiment, the carbon nitride precursor is fully mixed, including: firstly mixing by at least one of hydrothermal, stirring or shaking, and then drying by at least one of vacuum oven drying, heating evaporation drying, rotary evaporation drying or freeze drying. Before mechanical grinding, the selected one or more precursors are fully mixed to make the micro-polymerization process caused by the local high temperature during the mechanical grinding process more uniform.
[0038] In a preferred embodiment, the ball milling mode includes revolution, rotation, or a combination of revolution and rotation.
[0039] In a preferred embodiment, it also includes: calcining the sample obtained after ball milling by solid phase method, grinding, washing and drying to obtain the carbon nitride nanospheres; the atmosphere used in the solid phase method includes inert gas or static air, and the gas flow rate of the inert gas is 20-100 mL / min; the calcination temperature is 400-800℃; the calcination procedure includes heating to the target temperature in one step or heating to the target temperature in steps; the heating rate of calcination is 0.1-10℃ / min; the calcination time is 1-6h. Furthermore, the cooling process after high temperature calcination can be furnace cooling, slow cooling at room temperature, fast cooling with ice water or sudden cooling with liquid nitrogen; the drying process includes vacuum oven drying, heating evaporation, rotary evaporation drying or freeze drying.
[0040] The preparation method of the above carbon nitride nanospheres specifically includes:
[0041] (1) Weighing melamine and urea as carbon nitride precursors in a certain mixing mass ratio (1:1-1:20), and mixing them thoroughly by stirring and then freeze-drying;
[0042] (2) weighing a certain amount of NaCl in a certain mass ratio (5:1-1:5) and placing it together with the mixed precursor obtained in step (1) into a grinding jar;
[0043] (3) Similarly, pickaxe balls of a certain volume and combination are weighed according to the mass ratio (30:1-100:1) of the mixed precursor obtained in step (1), and are placed into a grinding jar together with the mixed precursor obtained in step (1) and the NaCl weighed in step (2);
[0044] (4) setting the ball milling time (1-6 h), ball milling mode and speed (200-500 r / min) to perform the ball milling operation in step (3);
[0045] (5) The sample obtained by mechanical grinding (i.e., step (4)) is then subjected to high-temperature calcination by a solid phase method, wherein the atmosphere is static air or an inert gas such as nitrogen or argon, the flow rate of the inert gas is 20-100 mL / min, and the calcination procedure is to heat the sample to a target temperature in one step, the target temperature is 400-800°C, the speed is 0.1-10°C / min, and the calcination time is 1-6 h;
[0046] (6) Grinding the sample obtained by calcining in step (5) into powder using a mortar;
[0047] (7) washing the powder obtained in step (6) with water to remove NaCl crystallites in the sample;
[0048] (8) Drying the sample washed with water in step (7) by freeze drying to obtain the carbon nitride nanospheres.
[0049] The present invention also provides a carbon nitride nano-microsphere, which is prepared by the preparation method of the carbon nitride nano-microsphere described in any of the above technical solutions. The carbon nitride nano-microsphere has the characteristics of high catalytic activity and good cycle performance.
[0050] Another aspect of the present invention provides the use of the carbon nitride nano-microspheres in the field of catalytic degradation and energy catalysis. Preferably, another aspect of the present invention provides the use of the carbon nitride nano-microspheres in the field of photocatalytic degradation of organic pollutants.
[0051] The present invention also provides a composite material, comprising the carbon nitride nano-microspheres described in any of the above technical solutions. Specifically, the composite material uses carbon nitride nano-microspheres as components, and is doped with metal ions or loaded with nanoparticles through an impregnation method, a coprecipitation method, an in-situ calcination method, an in-situ hydrothermal method, and is composited with a large specific surface area carrier, composited with a semiconductor as a co-catalyst, and constructed into a micro heterojunction to form a composite material with a two-dimensional morphology.
[0052] In order to more clearly and in detail introduce the carbon nitride nano-microspheres, preparation methods, applications and composite materials provided by the embodiments of the present invention, they will be described in conjunction with specific embodiments below.
[0053] Example 1
[0054] First, melamine and urea were mixed in a mass ratio of 1:5 by stirring and then freeze-drying. Subsequently, a certain amount of NaCl was weighed in a mass ratio of 1:3 to the mixed precursor and placed in a grinding jar together with the mixed precursor. Similarly, a combination of picks with a radius of 1-3 mm and a radius of 5-10 mm was weighed in a mass ratio (1:50) to the mixed precursor and placed in a grinding jar together with the mixed precursor and NaCl. Subsequently, the ball milling time was set to 2.5 h, the ball milling mode was combined with revolution and rotation, and the speed was 500 r / min for ball milling. Next, after the picks were screened out, the ball-milled precursor was heated to 550°C at a rate of 2.3°C / min under a nitrogen atmosphere (flow rate of 50 mL / min) and kept at high temperature for 4 h for calcination. After grinding, the obtained solid was washed with water and freeze-dried to obtain carbon nitride nanospheres.
[0055] Example 2
[0056] First, melamine and urea were mixed in a mass ratio of 1:5 by stirring and then freeze-drying. Subsequently, a certain amount of NaF was weighed in a mass ratio of 1:3 to the mixed precursor and placed in a grinding jar together with the mixed precursor. Similarly, a combination of picks with a radius of 1-3 mm and a radius of 5-10 mm was weighed in a mass ratio (1:50) to the mixed precursor and placed in a grinding jar together with the mixed precursor and NaF. Subsequently, the ball milling time was set to 2.5 h, the ball milling mode was combined with revolution and rotation, and the speed was 500 r / min for ball milling. Next, after the picks were screened out, the ball-milled precursor was heated to 550°C at a rate of 2.3°C / min under a nitrogen atmosphere (flow rate of 50 mL / min), and maintained at high temperature for 4 h for calcination. After grinding, the obtained solid was washed with water, and the carbon nitride catalyst of Example 2 was obtained by freeze drying.
[0057] Example 3
[0058] First, melamine and urea were mixed in a mass ratio of 1:5 by stirring and then freeze-drying. Subsequently, a certain amount of NaCl was weighed in a mass ratio of 1:3 to the mixed precursor and placed in a grinding jar together with the mixed precursor. Similarly, a combination of picks with a radius of 1-3 mm and a radius of 5-10 mm was weighed in a mass ratio (1:50) to the mixed precursor and placed in a grinding jar together with the mixed precursor and NaCl. Subsequently, the ball milling time was set to 0.5 h, the ball milling mode was combined with revolution and rotation, and the speed was 500 r / min for ball milling. Next, after the picks were screened out, the ball-milled precursor was heated to 550°C at a rate of 2.3°C / min under a nitrogen atmosphere (flow rate of 50 mL / min), and maintained for 4 h for high-temperature calcination. After grinding, the obtained solid was washed with water, and the carbon nitride catalyst of Example 3 was obtained by freeze drying.
[0059] Comparative Example 1
[0060] First, melamine and urea were mixed thoroughly in a mass ratio of 1:5 by stirring and then freeze-drying. Subsequently, a combination of picks with a radius of 1-3 mm and a radius of 5-10 mm was weighed in a mass ratio (1:50) with the mixed precursor, and placed in a grinding jar together with the mixed precursor. Subsequently, the ball milling time was set to 2.5 h, the ball milling mode was a combination of revolution and rotation, and the speed was 500 r / min for ball milling. Next, after the picks were screened out, the ball-milled precursor was heated to 550°C at a rate of 2.3°C / min under a nitrogen atmosphere (flow rate of 50 mL / min), and maintained for 4 h for high-temperature calcination. After grinding, the carbon nitride catalyst of Comparative Example 1 was obtained.
[0061] Comparative Example 2
[0062] First, melamine and urea were mixed in a mass ratio of 1:5 by stirring and then freeze-drying. Subsequently, a certain amount of NaCl was weighed in a mass ratio of 1:3 to the mixed precursor, and placed in an agate mortar together with the mixed precursor, and ground for one hour. Next, the mixed and ground precursor was heated to 550°C at a rate of 2.3°C / min under a nitrogen atmosphere (flow rate 50 mL / min), and maintained for 4 hours for high-temperature calcination. After grinding, the obtained solid was washed with water, and freeze-dried to obtain the carbon nitride catalyst of Comparative Example 2.
[0063] Comparative Example 3
[0064] First, melamine and urea were mixed in a mass ratio of 1:5 by stirring and then freeze-drying. Subsequently, the mixed precursor was heated to 550°C at a rate of 2.3°C / min under a nitrogen atmosphere (flow rate of 50 mL / min) and maintained for 4 hours for high-temperature calcination. After grinding, the carbon nitride catalyst of Comparative Example 3 was obtained.
[0065] Performance Testing
[0066] The carbon nitride catalysts of the examples and comparative examples were scanned by electron microscope. Figure 1-6 The X-ray diffraction pattern of the carbon nitride material prepared in Example 1 is shown in Figure 7 As shown, the electron paramagnetic resonance spectra of the carbon nitride materials prepared in Example 1 and Comparative Example 3 are as follows Figure 8 As shown. Figure 1-6 It can be seen from the figure that the morphological characteristics of the carbon nitride nanospheres obtained by the preparation method described in the present invention. In addition, the importance of sodium chloride combined with strong mechanical ball milling for the special morphology, the carbon nitride obtained without sodium chloride and ball milling process is tubular, the carbon nitride obtained without ball milling process is a multi-layer stacked morphology, and the carbon nitride obtained without sodium chloride is also tubular.
[0067] Conventional photocatalytic degradation experiment: The experiment was carried out at 25±2℃ with a xenon lamp simulating visible light irradiation (300 W Xe lamp, CEL-HXF 300, filter 420 nm). A 100 mL 20 mg / L tetracycline solution was placed in a photocatalytic reactor, the pH value of the solution was adjusted with 1 mol / L NaOH and HCl solution, and a specified amount of catalyst powder (0.25 g / L) was added. Stir continuously for 30 min in the dark to allow the system to reach adsorption and desorption equilibrium. Subsequently, a light source was added for irradiation to carry out the photocatalytic degradation reaction. Samples were taken at a specific reaction time, centrifuged, and the supernatant was taken for detection and the corresponding concentration was calculated to obtain the degradation efficiency.
[0068] Catalytic cycle test: The degradation rate of the catalyst detected by repeated experiments on organic pollutants is an important criterion for judging the stability of the catalyst. The catalyst dosage and other reaction conditions are kept consistent in repeated experiments. The catalyst collected through multiple degradation experiments can ensure that the catalyst dosage is sufficient after each cycle test. The specific experimental operation is as follows: After the catalytic test, solid-liquid separation is performed by centrifugation, and the catalyzed catalyst is washed multiple times with deionized water and alcohol, directly collected after vacuum drying, and then reused for degradation experiments. The specific catalytic experimental steps are the above-mentioned degradation experimental steps.
[0069] The conventional photocatalytic degradation results of Example 1 and Comparative Example 3 are as follows: Fig. 9 As shown in the figure, it can be seen that due to the special morphology of the nano-microspheres in Example 1, Example 1 shows the best photocatalytic degradation effect compared with Comparative Example 3, and its degradation activity for tetracycline is fully improved. At the same time, the cycle performance test of Example 1 was carried out ( Fig.10 ), Example 1 showed excellent recycling ability, which fully demonstrated its practical application potential in the field of water pollution control.
Claims
1. A method for preparing carbon nitride nanospheres, characterized in that: include: The carbon nitride precursor is fully mixed, microcrystals are added, and then ball milling is performed using a grinding body to obtain carbon nitride nanospheres; The carbon nitride precursor is a nitrogen-rich organic compound; the microcrystals are selected from one of halide salts, KSCN or Na2SO4; The radius of the grinding body is 1-3 mm; or the radius of the grinding body is 5-10 mm; or the grinding body is composed of a mixture of grinding bodies with a radius of 1-3 mm and grinding bodies with a radius of 5-10 mm; The ball milling speed is selected from any value between 200 and 500 r / min, and the ball milling time is selected from any value between 1 and 6 h; The nitrogen-rich organic compound is selected from a plurality of compounds selected from urea, cyanamide, dicyandiamide, melamine, thiourea, and dimethylformamide; The mass ratio of the microcrystals to the carbon nitride precursor is 5:1-1:
5.
2. The method for preparing carbon nitride nanospheres according to claim 1, characterized in that: The microcrystals are selected from one of halide salts, KSCN, or Na2SO4; and the grinding body is a pickaxe ball.
3. The method for preparing carbon nitride nanospheres according to claim 1, characterized in that: The nitrogen-rich organic compound is selected from melamine and urea, and the mixing mass ratio of the melamine to the urea is 1:1-1:
20.
4. The method for preparing carbon nitride nanospheres according to claim 1, characterized in that: The mass ratio of the carbon nitride precursor to the grinding body is 1:30-1:
100.
5. The method for preparing carbon nitride nanospheres according to claim 1, characterized in that: The step of fully mixing the carbon nitride precursor comprises: firstly mixing the carbon nitride precursor by at least one of hydrothermal, stirring or shaking, and then drying the carbon nitride precursor by at least one of vacuum oven drying, heating evaporation drying, rotary evaporation drying or freeze drying.
6. The method for preparing carbon nitride nanospheres according to claim 1, characterized in that: The ball milling modes include revolution, rotation, or a combination of revolution and rotation.
7. The method for preparing carbon nitride nanospheres according to claim 1, characterized in that: Also includes: The sample obtained after ball milling is calcined by a solid phase method, ground, washed with water and then dried to obtain the carbon nitride nanospheres; the atmosphere used in the solid phase method includes an inert gas or static air, and the gas flow rate of the inert gas is 20-100 mL / min; the calcination temperature is 400-800°C; the calcination procedure includes heating to the target temperature in one step or heating to the target temperature in steps; the calcination heating rate is 0.1-10°C / min; and the calcination time is 1-6 h.
8. A carbon nitride nanosphere, characterized in that: The carbon nitride nanospheres are prepared by the preparation method of any one of claims 1 to 7.
9. Use of the carbon nitride nanospheres according to claim 8 in the fields of catalytic degradation and energy catalysis.
10. A composite material, characterized in that: The invention comprises the carbon nitride nano-microspheres as described in claim 8.