A method for calculating the evaporation loss of rare earth elements in alloy smelting process

By calculating the evaporation loss of rare earth elements during alloy smelting, combined with Langmuir dynamics and Gibbs formula, the precise control problem of evaporation loss of rare earth elements in alloy smelting is solved, and the controllable preparation and use efficiency of rare earth content is achieved, which is in line with the Requirements for green and sustainable development.

CN118692583BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163823.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

In alloy smelting preparation, the evaporation loss of rare earth elements cannot be accurately controlled, making it difficult to prepare high-performance alloys with controllable rare earth content. The prior art cannot quantitatively calculate the correspondence between the evaporation loss and the addition amount of rare earths.

Method used

By calculating the surface area of ​​the alloy melt contacts the gas in the smelting equipment and the volatility rate of rare earth elements during the alloy smelting process, combining Langmuir dynamics and Gibbs formula, the evaporation loss of rare earth elements is quantitatively calculated, and a correction coefficient is introduced to correct the rare earth elements. Mole fraction, establish the relationship between the amount of rare earth addition and the amount of loss.

Benefits of technology

It has achieved precise control of the rare earth content, improved the efficiency of rare earth use, reduced the consumption of rare earth raw materials, and met the requirements of green and sustainable development of the industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118692583B_ABST
    Figure CN118692583B_ABST
Patent Text Reader

Abstract

The present invention provides a method for calculating the evaporation loss of rare earth elements in an alloy smelting process, which relates to the technical field of rare earth microalloying alloy preparation, and comprises the following steps: Step 1) calculating the surface area of ​​the alloy melt in contact with the gas in the smelting equipment during the alloy smelting process; S ; Step 2) Calculate the volatilization rate of rare earth element j in the i-th time element dt V j ; Step 3) According to the surface area of ​​the alloy melt in contact with the gas in the smelting equipment S and the volatilization rate of rare earth elements V j , calculate the loss d of rare earth elements in the i-th time element dt m i :Step 4) According to the loss of rare earth elements in the time element dt m i , calculate the loss of rare earth elements Δ within smelting time t m The present invention quantitatively calculates the evaporation loss of rare earth elements in the high-temperature alloy smelting process by citing the Langmuir kinetic calculation law of element evaporation and melt quality control theory and considering the time-varying volatilization of rare earth elements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth microalloying alloy preparation, and in particular relates to a method for accurately calculating the evaporation loss of rare earth elements in an alloy smelting process. Background Art

[0002] Rare earth elements (Y, Sc, lanthanide) as a super-active element have received special attention and wide application, especially rare earth Y, Ce, La added to alloys can significantly improve the material's resistance to high-temperature oxidation and corrosion resistance, and are widely used in various alloys as "vitamins" in alloys, and are important elements that are expected to break through the comprehensive performance of the new generation of high-temperature alloys. In addition to significantly improving the material's resistance to high-temperature oxidation and corrosion, rare earth elements have also made major breakthroughs in enhancing the mechanical properties of materials. For example, Y can significantly improve its creep properties in the research of high-strength bearing steel, cast stainless steel, magnesium / aluminum alloys, and high-temperature alloys. This shows that rare earth elements play an irreplaceable and important role in alloys.

[0003] However, despite the wide application of rare earths in various alloys, there are still many problems in the research of rare earth alloys. The most common and fundamental problem is the burning of rare earths during alloy smelting and preparation. The burning problem occurs in the first step of alloy smelting and preparation. The rare earth content cannot be accurately controlled, which makes it difficult to clearly reveal the mechanism of action of rare earths on alloys, causing greater troubles and difficulties in revealing the influence of rare earths on the structure and properties of alloys. Relevant personnel studied the loss of Y in the effect of yttrium and sulfur on the oxidation resistance of nickel-based single crystal high-temperature alloys and found that the recovery rate of rare earth Y only reached 10% of the added amount; the loss and distribution of rare earths in cast single crystal high-temperature alloys were studied, and it was found that the evaporation loss of rare earths was the main factor of rare earth loss.

[0004] Although existing technologies disclose methods for reducing rare earth loss and improving rare earth recovery, they are unable to quantitatively calculate the evaporation loss of rare earths, that is, they are unable to quantitatively establish the corresponding relationship between the amount added and the amount retained. Therefore, it is difficult to accurately control and compensate for rare earths, and thus it is difficult to prepare high-performance alloys with controllable rare earths. Summary of the invention

[0005] Therefore, the present invention provides a method for calculating the evaporation loss of rare earth elements during alloy smelting, the purpose of which is to quantitatively calculate the evaporation loss during alloy smelting and establish the relationship between the rare earth addition amount and the loss.

[0006] In order to solve the above problems, the present invention provides a method for calculating the evaporation loss of rare earth elements in an alloy smelting process, comprising the following steps:

[0007] Step 1) Calculate the surface area of ​​the alloy melt in contact with the gas in the smelting equipment during the alloy smelting processS ;

[0008] Step 2) Calculate the volatilization rate of rare earth element j in the i-th time element dt V j ;

[0009] Step 3) Based on the surface area of ​​the alloy melt in contact with the gas in the smelting equipment S and the volatilization rate of rare earth elements V j , calculate the loss d of rare earth elements in the i-th time element dt m i , the calculation formula is:

[0010] d m i = V j · S ·d t ;

[0011] Step 4) Based on the loss of rare earth elements in the time element dt m i , calculate the loss of rare earth elements within smelting time t m , the calculation formula is:

[0012] .

[0013] Furthermore, in step 2), the volatilization rate of the rare earth element is V j The calculation formula is:

[0014] ;

[0015] In the formula, α j is the activity of rare earth element j in the alloy melt; P j 0 is the saturated vapor pressure of pure rare earth solution, in Pa; M j is the molar mass of rare earth element j, in g / mol; R is the gas constant; T is the holding temperature of the alloy melt during the smelting process, in K.

[0016] Furthermore, the activity of the rare earth element j in the alloy melt is α j The calculation formula is:

[0017] α j = c j · x j ;

[0018] In the formula, γ j is the activity coefficient of rare earth element j in the alloy melt; j is the molar fraction of rare earth element j.

[0019] Furthermore, the activity coefficient of the rare earth element j in the alloy melt is c j The calculation formula is:

[0020] ;

[0021] In the formula, is the excess partial molar free energy, in kJ / mol; c j is 1.

[0022] Furthermore, the correction factor K is introduced to j The correction coefficient K is calculated as follows:

[0023] ;

[0024] In the formula, N layer It is the amount of material in the excess layer on the surface of the alloy melt, in mol; N inter It is the amount of substance inside the alloy melt, in mol; is the volume of the excess layer on the surface of the alloy melt; is the volume inside the alloy melt.

[0025] Furthermore, the amount of material in the excess layer on the surface of the alloy melt is N layer The calculation formula is:

[0026] ;

[0027] Where d is the thickness of the excess layer, in units of ;

[0028] is the surface excess of rare earth element j, in mol / cm 2 , The calculation formula is:

[0029] ;

[0030] in, is the surface tension of the alloy melt, in mN / m; a is the concentration in the rare earth alloy solution, in mol / L.

[0031] Furthermore, the amount of the substance in the alloy melt is N inter The calculation formula is:

[0032] N inter = m j / M j ;

[0033] In the formula, m j is the set addition amount of rare earth element j in the alloy, in g.

[0034] On the other hand, the present invention also provides a smelting method of a rare earth alloy to smelt the alloy raw material, wherein the amount of rare earth elements added to the alloy raw material is the sum of the set amount of rare earth elements added to the rare earth alloy and the evaporation loss of the rare earth elements during the smelting process;

[0035] The evaporation loss of the rare earth element during the smelting process is obtained by using any of the calculation methods described above.

[0036] The method for calculating the evaporation loss of rare earth elements in the alloy smelting process provided by the present invention has the following beneficial effects:

[0037] 1. The present invention refers to the Langmuir kinetic calculation law of element evaporation and melt quality control theory, considers the change of volatilization of rare earth elements over time, quantitatively calculates the evaporation loss of rare earth elements in the high-temperature alloy smelting process, and reflects the change relationship between the concentration of rare earth elements and the smelting time, so as to accurately control and compensate the rare earth content in the alloy, guide the preparation of rare earth alloys with controllable rare earth content, and greatly improve the use efficiency of rare earths, reduce the consumption of rare earth raw materials, and achieve the requirements of green and sustainable industrial development.

[0038] 2. When calculating the loss of rare earth elements, the present invention corrects the molar fraction of rare earth elements based on the special physical properties of surface adsorption of rare earth elements. The correction ensures that the calculation of rare earth loss is more accurate, so as to prepare alloys with more accurate rare earth content. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0040] Figure 1 A graph showing the rare earth recovery rate of DD5 alloy obtained by using the calculation model of the present application and the corresponding experimental data;

[0041] Figure 2 This is a composition detection diagram of the surface and core element Y of the sample containing 0.5wt% Y in the example. DETAILED DESCRIPTION

[0042] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0043] The present invention quantitatively analyzes the relationship between the change of rare earth concentration in alloys with time by citing the kinetic calculation law of element evaporation, and introduces the special physical properties of surface adsorption of rare earth elements to perform concentration compensation in the calculation process of rare earth element evaporation loss. From the perspective of theoretical mechanism, the actual process and loss of rare earth element evaporation are revealed and calculated, which not only establishes a clear relationship between the amount of rare earth added and the amount of retained, but also greatly improves the use efficiency of rare earth, laying a theoretical basis and foundation for further clarifying the distribution law of rare earth in alloys and revealing the comprehensive performance of rare earth strengthened alloys.

[0044] The specific scheme of the present invention is as follows:

[0045] A method for calculating the evaporation loss of rare earth elements in an alloy smelting process comprises the following steps:

[0046] Step 1) Calculate the surface area of ​​the alloy melt in contact with the gas in the smelting equipment during the alloy smelting process S ;

[0047] Step 2) Calculate the volatilization rate of rare earth element j in the i-th time element dt V j ;

[0048] Step 3) Based on the surface area of ​​the alloy melt in contact with the gas in the smelting equipment S and the volatilization rate of rare earth elements V j, combined with the Langmuir theoretical formula for interface melt quality control, calculate the loss of rare earth elements d in the i-th time element dt m i , the calculation formula is:

[0049] d m i = V j · S ·d t ;

[0050] Step 4) Based on the loss of rare earth elements in the time element dt m i , calculate the loss of rare earth elements within smelting time t m , the calculation formula is:

[0051] .

[0052] Based on the above method, S The size is related to the inner cavity of the smelting equipment. For example, in a directional solidification furnace, only the top of the alloy melt contacts the gas and evaporates, so the contact surface can be approximately circular. Considering the volatilization rate of rare earth elements V j Changing with time t can ensure that the calculated loss amount is more accurate.

[0053] In some embodiments, in step 2), the volatilization rate of the rare earth element is V j The calculation formula is:

[0054] ;

[0055] In the formula, α j is the activity of rare earth element j in the alloy melt; P j 0 is the saturated vapor pressure of pure rare earth solution, in Pa, which can be obtained by looking up the surface tension handbook of metals and alloys; M j is the molar mass of rare earth element j, in g / mol; R is the gas constant; T is the holding temperature of the alloy melt during the smelting process, in K.

[0056] In some embodiments, the activity of the rare earth element j in the alloy melt is α j The calculation formula is:

[0057] α j = c j · x j ;

[0058] In the formula, γ j is the activity coefficient of rare earth element j in the alloy melt; j is the molar fraction of rare earth element j.

[0059] In some embodiments, the activity coefficient of the rare earth element j in the alloy melt is c j The calculation formula is:

[0060] ;

[0061] In the formula, is the excess partial molar free energy, in kJ / mol;

[0062] c j is 1. Since the rare earth content in the alloy is relatively low and its concentration is also very low, the alloy solution (alloy melt) containing rare earth can be regarded as a dilute solution of rare earth, so the activity coefficient is regarded as 1.

[0063] The surface excess concentration causes the concentration of rare earth elements at the liquid / gas interface to be significantly higher than that inside the liquid metal, so that there is an excess layer of a certain thickness at the gas / liquid interface of the alloy melt, which is the surface excess layer. In some embodiments, the Gibbs formula for calculating the surface excess of the solution is used, and a correction coefficient K is introduced to the x j After the correction factor K is introduced, the volatilization rate of rare earth element j is V j The calculation formula is:

[0064] ;

[0065] The calculation formula of the correction coefficient K is:

[0066] ;

[0067] In the formula, N layer It is the amount of material in the excess layer on the surface of the alloy melt, in mol; N inter It is the amount of substance inside the alloy melt, in mol; is the volume of the excess layer on the surface of the alloy melt; is the volume inside the alloy melt.

[0068] The ratio of the amount of substance in the excess layer per unit volume to the amount of substance in the internal alloy liquid per unit volume, that is, the ratio K of the liquid surface and internal concentrations, is obtained and converted into a molar fraction.

[0069] In some embodiments, the amount of material in the surface excess layer is N layer The calculation formula is:

[0070] ;

[0071] Where d is the thickness of the excess layer on the surface, in units of ;

[0072] is the surface excess of rare earth element j, in mol / cm 2 , The calculation formula is:

[0073] ;

[0074] in, The excess amount of rare earth element j in the surface layer of the alloy melt compared to the equivalent amount of bulk phase inside; A is the surface area of ​​the alloy melt, in cm 2 ; is the surface tension of the alloy melt, in mN / m; a is the concentration in the rare earth alloy solution, in mol / L.

[0075] In some embodiments, the amount of the substance in the alloy melt is N inter The calculation formula is:

[0076] N inter = m j / M j ;

[0077] In the formula, m j is the set addition amount of rare earth element j in the alloy, in g.

[0078] On the other hand, the present invention also provides a smelting method of a rare earth alloy, wherein the alloy raw material is smelted to obtain an actual content of rare earth in the rare earth alloy close to the set addition amount; wherein the addition amount of rare earth elements in the alloy raw material (i.e., the actual addition amount) is the sum of the set addition amount of rare earth elements in the rare earth alloy and the evaporation loss amount of the rare earth elements during the smelting process; the set addition amount of rare earth elements is the required content of rare earth in the pre-prepared rare earth alloy, i.e., the expected retention amount of rare earth; the actual content of rare earth is the content of rare earth in the finally prepared rare earth alloy;

[0079] The evaporation loss of the rare earth element is obtained by using any of the calculation methods described above.

[0080] The present invention will be further described below in conjunction with specific embodiments.

[0081] Example

[0082] This embodiment provides a method for calculating the evaporation loss of rare earth elements during alloy smelting. The alloy is a DD5 alloy with rare earth Y added. The composition of the alloy is shown in Table 1 in terms of mass percentage. The contents of rare earth Y are 0.01wt.%, 0.05wt.%, 0.2wt.%, and 0.5wt.%. During the smelting process, the holding temperature is set at 1550°C and the initial vacuum is evacuated for 10 -3 Pa, and then filled with argon gas to 10 5 Pa, and the holding time is 1min, 5min, and 15min respectively.

[0083] Table 1 Composition (wt%) of the alloy (DD5) used in the examples of the present invention

[0084]

[0085] The calculation method specifically includes the following steps:

[0086] Step 1) Calculate the surface area of ​​the alloy melt in contact with the gas in the smelting equipment during the alloy smelting process S In this embodiment, S is the surface area of ​​the vaporizable droplet in the optical levitation experiment, which is approximately the surface area of ​​a sphere. S =4πr 2 , r=5mm;

[0087] Step 2) Calculate the volatilization rate of rare earth element Y in the i-th time element dt V Y ; The calculation formula is:

[0088] ;

[0089] Among them, the query P Y 0 =0.01Pa; M Y =88.906g / mol; R=8.314J / (mol*k); T=1550K.

[0090] α Y = c Y · xY ;

[0091] Among them, γ Y ≈1; for the four components, χ Y They are: Y =6.75556E-05 (when Y=0.01wt.%), χ Y =3.37963E-04 (when Y=0.05wt.%), χ Y =1.354641E-03(when Y=0.2wt.%), χ Y =3.400627E-03 (when Y=0.5wt.%);

[0092] The GYbbs formula for surface excess calculation of the solution is used, and the correction factor K is introduced to χ Y After correction, the excess GYbbs formula of the solution surface is:

[0093] ;

[0094] For the four components, the tested and calculated , a and The values ​​are =1610.528mN / m, a=0.1333mol / L, =1.29E-05mol / dm 2 (When Y=0.01wt.%), =1602.214mN / m, a=0.6663mol / L, =2.51E-05mol / dm 2 (When Y=0.05wt.%), =1591.035mN / m, a=2.5563mol / L, =1.03E-04mol / dm 2 (When Y=0.2wt.%), =1573.663mN / m, a=6.6632mol / L, =2.62E-04mol / dm 2 (When Y = 0.5wt.%);

[0095] The calculation formula of the correction coefficient K is:

[0096] ;

[0097] In the formula, ≈4 / 3πr 3 ; ≈4πr 2 ·d;N layer = 4πR 2 ·d; measured d≈2um; N Ynter = m Y / M Y ;

[0098] in, M Y =88.906 g / mol; for the four components, m Y They are: m Y =0.05g (when Y=0.01wt.%), m Y =0.25g (when Y=0.05wt.%), m Y =1g (when Y=0.2wt.%), m Y =2.5g (when Y=0.5wt.%);

[0099] Volatilization rate of rare earth element Y after introducing correction factor K V Y The calculation formula is:

[0100] ;

[0101] Step 3) Based on the surface area of ​​the alloy melt in contact with the gas in the smelting equipment S and the volatilization rate of rare earth elements V j , combined with the Langmuir theoretical formula for interface melt quality control, calculate the loss of rare earth elements d in the i-th time element dt m i , the calculation formula is:

[0102] d m i = V Y · S ·d t ;

[0103] Step 4) Based on the loss of rare earth elements in the time element dt m i , calculate the loss of rare earth elements within smelting time t m , the calculation formula is:

[0104] .

[0105] The rare earth loss for holding times of 1 min, 5 min and 15 min was calculated respectively. The calculation results are shown in Table 2.

[0106] Among them, the composition detection (EDS-SEM) of element Y on the surface and core of the sample is as follows Figure 2 It can be seen that there is an adsorption layer with a high rare earth Y content on the surface of the sample, which confirms the phenomenon of active rare earth elements adsorbed on the surface of the liquid. The adsorption phenomenon changes the concentration of Y on the liquid surface, directly affecting the evaporation dynamics of rare earth Y, further verifying the necessity of using K value to compensate for the concentration of rare earth Y on the surface in this application.

[0107] The accuracy of the calculation method of the present application is verified by the optical suspension zone melting experiment method. The specific steps are: the button-shaped alloy ingots corresponding to the four components in the embodiment are obtained by the optical suspension zone melting equipment, the entire button ingot is cut into chips, and divided into three parts on average, and the rare earth Y composition is analyzed three times by chemical analysis. The three chemical analyses are used because the experimental data is measured only once, and the error is large. Measuring three times and averaging can more accurately measure the actual composition of the alloy. The final rare earth loss is shown in Table 2.

[0108] From Table 2 and Appendix Figure 1 It can be seen that the rare earth loss calculated by the method of the present application is highly consistent with the experimental results, which further verifies the effectiveness and reliability of the calculation method of the present application.

[0109] Table 2 Results of rare earth loss calculated and tested in Example

[0110]

[0111] Comparative Example

[0112] This comparative example provides a method for calculating the evaporation loss of rare earth elements during alloy smelting. The alloy is a DD5 alloy with rare earth Y added. The composition of the alloy is shown in Table 1 in terms of mass percentage, wherein the content of rare earth Y is 0.01wt.%, 0.05wt.%, 0.2wt.%, and 0.5wt.%. During the smelting process, the holding temperature is set at 1550°C, and the initial vacuum is evacuated for 10 -3 Pa, and then filled with argon gas to 10 5 Pa, the holding time is 1min, 5min, and 15min respectively. The calculation method specifically includes the following steps:

[0113] Step 1) Calculate the surface area of ​​the alloy melt in contact with the gas in the smelting equipment during the alloy smelting process S In this implementation S is the surface area of ​​the vaporizable droplet in the optical levitation experiment, which is approximately the surface area of ​​a sphere.S =4πr 2 , r=5mm;

[0114] Step 2) Calculate the volatilization rate of the rare earth element in the i-th time element dt V Y ; The calculation formula is:

[0115] ;

[0116] Among them, the query P Y 0 =0.01Pa; M Y =88.906g / mol; R=8.314J / (mol*k); T=1550K.

[0117] α Y = c Y · x Y ;

[0118] Among them, γ Y ≈1; for the four components, χ Y They are: Y =6.75556E-05 (when Y=0.01wt.%), χ Y =3.37963E-04 (when Y=0.05wt.%), χ Y =1.354641E-03(when Y=0.2wt.%), χ Y =3.400627E-03 (when Y=0.5wt.%);

[0119] Step 3) Based on the surface area of ​​the alloy melt in contact with the gas in the smelting equipment S and the volatilization rate of rare earth elements V j , combined with the Langmuir theoretical formula for interface melt quality control, calculate the loss of rare earth elements d in the i-th time element dt m i , the calculation formula is:

[0120] d m i = V Y · S ·d t ;

[0121] Step 4) Based on the loss of rare earth elements in the time element dt mi , calculate the loss of rare earth elements Δ within smelting time t m , the calculation formula is:

[0122] .

[0123] The rare earth loss at holding times of 1 min, 5 min and 15 min was calculated respectively. The results are shown in Table 3.

[0124] Table 3 Results of rare earth loss calculated by comparative example

[0125]

[0126] In this comparative example, the Langmuir kinetic model of rare earth concentration was not corrected with K value, and the parameters used in the model calculation were exactly the same as those in the embodiment, and the calculated rare earth loss was poorly consistent with the experimental results. As can be seen from Tables 2 and 3, the calculated results of the evaporation loss of the comparative example are seriously smaller than the experimental results. This shows that the Langmuir model without considering the surface excess is not suitable for the loss calculation of rare earth elements with adsorption phenomenon. The surface excess phenomenon directly and significantly increases the content of rare earth on the surface of the alloy melt, and the content is a key parameter affecting evaporation in liquid metal. The higher the content, the greater the driving force for evaporation, indicating that the surface excess of rare earth is a key factor in determining the evaporation loss of rare earth, verifying the effectiveness and reliability of the calculation method of this application. The occurrence of the rare earth surface excess phenomenon is due to the fact that rare earths have very low surface tension. In order to further reduce the total energy, the liquid metal forces rare earth atoms to enrich on the surface of the alloy melt, thereby reducing the surface tension of the alloy in order to obtain lower total energy.

[0127] The above is only a specific implementation method of the present invention for DD5 rare earth Y nickel-based high-temperature alloy, and is also applicable to other rare earths (Ce, Sc, La, etc.) and alloys. It is only necessary to adjust the physical parameters corresponding to the specific rare earth elements and the various physical parameters in the formula. However, the protection scope of the present invention is not limited to this. Any technician familiar with the technical field within the technical scope disclosed by the present invention, according to the technical solution and inventive concept of the present invention, replaces the rare earth elements, alloy types or adjusts the experimental parameters by equivalent substitution, which should be covered within the protection scope of the present invention.

[0128] The present invention starts from solving the scientific problem of rare earth loss in the smelting process, adopts the intersection of multiple disciplines such as melt quality control in the material smelting process, chemical properties of surfactant materials, and physical and chemical properties, comprehensively and deeply grasps the special behavior of rare earth elements on the surface / interior of the molten alloy and in the smelting process, and solves the long-standing problem of rare earth burning loss that can only be qualitative but not quantitative through the optimization of theoretical calculation models. It lays a theoretical basis and foundation for further clarifying the distribution law of rare earths in alloys and revealing the comprehensive performance of rare earth-strengthened alloys. At the same time, the present invention successfully establishes the corresponding relationship between the amount of rare earth added and the yield, greatly improves the use efficiency of rare earths, and reduces the consumption of raw materials for rare earths. The present invention meets the requirements of current industrial green and sustainable development.

[0129] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.

[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A method for calculating the evaporation loss of rare earth elements in an alloy smelting process, characterized in that: The following steps are involved: Step 1) Calculate the surface area of ​​the alloy melt in contact with the gas in the smelting equipment during the alloy smelting process S ; Step 2) Calculate the volatilization rate of rare earth element j in the i-th time element dt V j ; Step 3) Based on the surface area of ​​the alloy melt in contact with the gas in the smelting equipment S and the volatilization rate of rare earth elements V j , calculate the loss d of rare earth elements in the i-th time element dt m i , the calculation formula is: d m i = V j · S ·d t ; Step 4) Based on the loss of rare earth elements in the time element dt m i , calculate the loss of rare earth elements within smelting time t m , the calculation formula is: m = ; Wherein, in the step 2), the volatilization rate of the rare earth element is V j The calculation formula is: V j = α j · P j 0 · ; In the formula, α j is the activity of rare earth element j in the alloy melt; P j 0 is the saturated vapor pressure of pure rare earth solution, in Pa; M j is the molar mass of rare earth element j, in g / mol; R is the gas constant; T is the holding temperature of the alloy melt during the smelting process, in K; The activity of the rare earth element j in the alloy melt is α j The calculation formula is: α j = γ j · χ j ; In the formula, γ j is the activity coefficient of rare earth element j in the alloy melt; j is the molar fraction of rare earth element j; Introducing the correction factor K to χ j The calculation formula of the correction coefficient K is: K = N layer · / N inter ; In the formula, N layer It is the amount of material in the excess layer on the surface of the alloy melt, in mol; N inter It is the amount of substance inside the alloy melt, in mol; is the volume of the excess layer on the surface of the alloy melt; is the volume inside the alloy melt; The amount of material in the excess layer on the surface of the alloy melt N layer The calculation formula is: N layer = · S · d ; Where d is the thickness of the excess layer on the surface, in units of is the surface excess of rare earth element j, in mol / cm 2 , The calculation formula is: = ; in, is the surface tension of the alloy melt, in mN / m; a is the concentration in the rare earth alloy solution, in mol / L; The amount of material inside the alloy melt N inter The calculation formula is: N inter = m j / M j ; In the formula, m j is the set addition amount of rare earth element j in the alloy, in g.

2. The method for calculating the evaporation loss of rare earth elements in the alloy smelting process according to claim 1, characterized in that: The activity coefficient of the rare earth element j in the alloy melt is γ j The calculation formula is: γ j =exp( / RT); In the formula, is the excess partial molar free energy, in kJ / mol; Said γ j is 1.

3. A method for smelting a rare earth alloy, characterized in that: The alloy raw material is smelted, and the amount of rare earth elements added to the alloy raw material is the sum of the set amount of rare earth elements added to the rare earth alloy and the evaporation loss of the rare earth elements during the smelting process; The evaporation loss of the rare earth element during the smelting process is obtained by using the calculation method described in any one of claims 1 or 2.