Method for preparing a jacket made of multifunctional fiber composite fabric
By using coaxial spinning of cellulose and polyimide in the jacket, ultrasonic treatment and spraying of nylon 66 to form a hollow structure, the problem of viscosity mismatch between polyimide and nylon 66 during spinning is solved, and the problem of improved viscosity is improved The warmth and mechanical properties of the jacket.
Patent Information
- Application Number
- CN202411187404.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The warmth and mechanical properties of existing jackets are insufficient. The viscosity and surface tension of polyimide and nylon 66 do not match during coaxial spinning, resulting in the inability to achieve a stable spinning effect.
Cellulose as the core fiber and polyimide as the outer fiber are coaxially spinned, and the hollow structure is formed by ultrasonic treatment and alkali solution soaking, and then spraying nylon 66 solution to form hollow polyimide composite fibers. Spinning and weaving, combined with polyimide yarn and polyvinyl alcohol yarn, to create a multifunctional fiber composite fabric.
The warm and mechanical properties of the fiber are improved, the warm and mechanical properties of the jacket are enhanced, and the problems of insufficient warm and mechanical properties of the jacket are solved in the prior art.
Smart Images

Figure CN118697126B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabric preparation, in particular to a multi-component woven fabric, and in particular to a method for preparing a jacket made of a multifunctional fiber composite fabric. Background Art
[0002] A windbreaker, also known as a windbreaker or raincoat, is an outdoor sports equipment designed to provide protection during outdoor adventures, hiking, mountaineering, skiing and other activities. It combines multiple functions such as waterproofing, breathability, and warmth to cope with complex and changeable outdoor environments.
[0003] Polyimide is a type of high molecular polymer containing cyclic imide groups in the molecular chain. It is one of the organic polymer materials with the best comprehensive performance. Its characteristics include high temperature resistance, high insulation performance, good mechanical properties, excellent weather resistance, corrosion resistance, etc. Due to its unique properties, polyimide has gradually been used in the field of outdoor clothing. In particular, its high thermal insulation, flame retardancy, high and low temperature resistance and other characteristics make polyimide fiber an ideal material for outdoor clothing such as assault jackets.
[0004] Nylon 66 is a translucent or opaque milky white crystalline polymer with the characteristics of plasticity, excellent heat resistance, chemical resistance and strength. The high strength and wear resistance of nylon 66 make it an ideal choice for making jacket fabrics. It can resist scratches and wear in outdoor environments and maintain the integrity and durability of clothing.
[0005] Coaxial spinning of polyimide and nylon 66 to form coaxial fibers can combine the high thermal insulation of polyimide and the high mechanical properties of nylon 66, making the jacket have good thermal insulation and mechanical strength. However, due to the mismatch in viscosity and surface tension between polyimide and nylon 66, a stable coaxial spinning effect cannot be achieved.
[0006] Therefore, it is necessary to improve the composite fabric jacket in the prior art to solve the above problems. Summary of the invention
[0007] The present invention overcomes the deficiencies of the prior art and provides a method for preparing a jacket made of a multifunctional fiber composite fabric, aiming to solve the defects of the jacket in the prior art, that is, insufficient warmth retention and mechanical properties.
[0008] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a jacket made of a multifunctional fiber composite fabric, comprising the following steps:
[0009] S1: Coaxial spinning of cellulose as core fiber and polyimide as outer fiber to obtain original polyimide fiber;
[0010] S2: treating the original polyimide fiber with ultrasound and then immersing the fiber in an alkaline solution to obtain a hollow polyimide fiber;
[0011] S3: spraying nylon 66 solution onto the surface of the hollow polyimide fiber to obtain a hollow polyimide composite fiber;
[0012] S4: spinning the hollow polyimide composite fiber to obtain polyimide yarn, and weaving the polyimide yarn as warp yarn and polyvinyl alcohol yarn as weft yarn to obtain a multifunctional fiber composite fabric;
[0013] S5: combining the multifunctional fiber composite fabric with the outer layer of the jacket to obtain a jacket made of multifunctional fiber composite fabric.
[0014] In a preferred embodiment of the present invention, the coaxial spinning method in S1 is to spin the cellulose spinning solution and the polyimide spinning solution using a coaxial spinning device, the extrusion speed of the cellulose spinning solution is 7-9 ml / min, the extrusion speed of the polyimide spinning solution is 3-5 ml / min, the diameter of the core layer fiber is 4-8 μm, and the outer diameter of the outer layer fiber is 12-16 μm.
[0015] In a preferred embodiment of the present invention, the mass fraction of the solvent in the cellulose spinning solution is 55-65%, the solvent is ethanol, the mass fraction of ethanol is 85-95%, the mass fraction of polyimide in the polyimide spinning solution is 20%-30%, and the solvent is N,N-dimethylacetamide.
[0016] In a preferred embodiment of the present invention, the frequency of the ultrasonic treatment in S2 is 30-50 Hz, and the treatment time is 20-40 min.
[0017] In a preferred embodiment of the present invention, the main component of the alkaline solution in S2 is sodium hydroxide, the concentration of the alkaline solution is 10-20%, and the soaking time is 1-1.5h.
[0018] In a preferred embodiment of the present invention, the fiber is stretched during the soaking in the alkaline solution in S2, the stretching ratio is 1:2-4, and the stretching direction is along the fiber axis.
[0019] In a preferred embodiment of the present invention, the nylon 66 solution in S3 contains: nylon 66, formic acid and adhesive, the mass ratio of the nylon 66, the formic acid and the adhesive is: 15-20:70-85:1-2, and the spraying time is 20-30min.
[0020] In a preferred embodiment of the present invention, after spraying the nylon 66 solution on the surface of the hollow polyimide fiber and forming a nylon 66 fiber layer in S3, the hollow polyimide fiber is immersed in a polytetrafluoroethylene solution for 0.5-1h, and the mass fraction of the polytetrafluoroethylene is 20-30%.
[0021] In a preferred embodiment of the present invention, the fineness of the polyimide yarn in S4 is 40-60D, the fineness of the polyvinyl alcohol yarn is 30-50D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 20-30F and 15-20F respectively, and the warp and weft densities of the multifunctional fiber composite fabric are 40-50 strands / cm and 55-60 strands / cm respectively.
[0022] In a preferred embodiment of the present invention, the multifunctional fiber composite fabric in S5 is combined with the outer layer of the jacket by sewing or bonding.
[0023] The present invention solves the defects existing in the background technology and has the following beneficial effects:
[0024] (1) The present invention provides a method for preparing a jacket made of a multifunctional fiber composite fabric, wherein cellulose and polyimide are made into coaxial fibers, and the coaxial fibers are subjected to ultrasonic treatment and alkali treatment in sequence, and nylon 66 is sprayed on the fiber surface, and the obtained fibers are spun and woven to form a jacket, so that polyimide and nylon 66 can form coaxial hollow fibers. Compared with the jacket in the prior art, polyimide and nylon 66 can be tightly combined with nylon 66 to form a hollow structure, and the thermal insulation performance and mechanical properties of the multifunctional fiber are improved, and the thermal insulation performance and mechanical properties of the jacket are enhanced, thereby solving the defects of the jacket in the prior art that the thermal insulation performance and mechanical properties are insufficient.
[0025] (2) In the present invention, the original polyimide fiber is treated with ultrasound and then immersed in an alkaline solution, which increases the mechanical bite between the cellulose fiber and the polyimide fiber, so that after the cellulose fiber is dissolved, part of the cellulose fiber remains on the inner side of the polyimide fiber. Compared with the prior art, the retained and evenly distributed cellulose fiber can serve as a supporting structure to improve the mechanical strength of the polyimide, and can slow down the heat transfer efficiency and improve the thermal insulation performance.
[0026] (3) In the present invention, cellulose and polyimide are made into coaxial fibers, the cellulose fibers are dissolved, and a nylon 66 coating is attached to the polyimide fibers, so that the hollow polyimide composite fibers can form hollow fibers on the polyimide fibers while ensuring the combination of polyimide and nylon 66. Compared with the prior art, the hollow structure improves the thermal insulation and mechanical properties of the fibers, and the combination of polyimide and nylon 66 further improves the thermal insulation and mechanical properties of the fibers.
[0027] (4) In the present invention, the original polyimide fiber is stretched during the soaking process in the alkaline solution, and the stretching direction is along the fiber axis. Compared with the prior art, the stretching process can make the fiber molecular chains arranged more neatly along the fiber axis, thereby improving the orientation degree of the fiber. The improvement of the orientation degree can increase the tensile strength and modulus of the fiber, thereby enhancing the mechanical properties of the fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 It is a method step diagram of a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0032] like Figure 1 As shown, a method for preparing a jacket made of a multifunctional fiber composite fabric comprises the following steps:
[0033] S1: Coaxial spinning is performed using cellulose as core fiber and polyimide as outer fiber to obtain raw polyimide fiber.
[0034] The coaxial spinning method in S1 is to spin cellulose spinning solution and polyimide spinning solution using a coaxial spinning device. The extrusion speed of the cellulose spinning solution is 7-9 ml / min, the extrusion speed of the polyimide spinning solution is 3-5 ml / min, the diameter of the core layer fiber is 4-8 μm, and the outer diameter of the outer layer fiber is 12-16 μm.
[0035] By setting the specific extrusion speed of cellulose spinning solution and polyimide spinning solution, the diameter size of the core fiber and the outer fiber can be precisely controlled to ensure the uniformity and consistency of the fiber structure. The diameter size ratio setting of the core and outer fibers helps to improve the mechanical bite between the two. Due to the ultrasonic treatment, the microscopic contact points between the fibers undergo local wear and reorganization, thereby promoting a tighter bond.
[0036] The mass fraction of the solvent in the cellulose spinning solution is 55-65%, the solvent is ethanol, and the mass fraction of the ethanol is 85-95%. The mass fraction of the polyimide in the polyimide spinning solution is 20%-30%, and the solvent is N,N-dimethylacetamide.
[0037] S2: The original polyimide fiber is treated with ultrasound and then immersed in an alkaline solution to obtain a hollow polyimide fiber.
[0038] The frequency of ultrasonic treatment in S2 is 30-50Hz, and the treatment time is 20-40min. The high-frequency vibration energy generated by ultrasonic waves can penetrate the liquid medium and act on the fiber surface, causing local wear and reorganization of the microscopic contact points between the fibers, thereby increasing the mechanical bite between the fibers and promoting a tighter combination of the core layer fibers and the outer layer fibers.
[0039] After the core fiber and the outer fiber are more tightly combined, when the alkaline solution dissolves the cellulose fiber, cellulose fiber will remain on the inner wall of the outer fiber. Since the ultrasonic treatment is uniform, the remaining cellulose fiber is evenly distributed. During the heat transfer process of air-cellulose fiber-polyimide fiber, it helps to maintain the temperature gradient inside the fiber and improve the thermal insulation performance. The remaining cellulose fiber can act as a "skeleton" to provide additional support when the polyimide fiber is subjected to external force, reduce the deformation or rupture of the fiber, and enhance the mechanical strength of the polyimide fiber. Ultrasonic treatment can also eliminate defects inside the fiber, such as bubbles and holes, improve the density and uniformity of the fiber, and thus enhance its mechanical strength.
[0040] Ultrasonic treatment can promote the rearrangement and combination of polymer chains inside the fiber, thereby enhancing the mechanical strength of the fiber, and the roughness of the outer surface of the outer fiber will increase, so that when the hollow polyimide fiber is subsequently combined with nylon 66, the binding property of the polyimide molecule and nylon 66 is enhanced, thereby improving the bonding strength between the hollow polyimide fiber and the nylon 66 fiber layer, and improving the mechanical strength of the hollow polyimide composite fiber.
[0041] The main component of the alkaline solution in S2 is sodium hydroxide, the concentration of the alkaline solution is 10-20%, and the soaking time is 1-1.5 hours. The sodium hydroxide concentration of 10-20% is relatively mild, which can effectively dissolve the cellulose fibers, while reducing the chemical damage to the outer layer of the polyimide fibers, and can avoid the cellulose fibers that are tightly combined with the inner wall of the polyimide hollow fiber. Alkaline solution treatment can improve the surface properties of the polyimide fiber, increase the surface roughness and change the surface charge, which helps to improve the bonding strength of the polyimide fiber when combined with the subsequent nylon 66.
[0042] In S2, the fiber is stretched during the soaking process in the alkaline solution, with a stretching ratio of 1:2-4 and a stretching direction along the fiber axis. The stretching process can make the fiber molecular chains more neatly arranged along the fiber axis, improve the orientation of the fiber, and the improvement of the orientation can increase the tensile strength and modulus of the fiber, thereby enhancing the mechanical properties of the fiber.
[0043] The stretching process can further refine the diameter of the fiber and make its shape more uniform. It helps the subsequent uniform coating of the nylon 66 solution, ensuring the consistency and functionality of the composite fiber surface. The stretched fiber has higher strength and stability, and is less likely to deform or break during the process of dissolving the B fiber to form a hollow structure, which helps maintain the integrity and uniformity of the hollow structure and further improves the breathability and warmth of the fabric.
[0044] S3: spraying nylon 66 solution onto the surface of the hollow polyimide fiber to obtain the hollow polyimide composite fiber.
[0045] The nylon 66 solution in S3 contains: nylon 66, formic acid and adhesive, the mass ratio of nylon 66, formic acid and adhesive is: 15-20:70-85:1-2, and the spraying time is 20-30 minutes. As a high-strength polymer, the addition of nylon 66 can significantly improve the breaking strength and wear resistance of the fiber, thereby enhancing the mechanical properties of the fiber.
[0046] In S3, after spraying nylon 66 solution on the surface of the hollow polyimide fiber to form a nylon 66 fiber layer, the hollow polyimide fiber is immersed in a polytetrafluoroethylene solution for 0.5-1h, and the mass fraction of polytetrafluoroethylene is 20-30%. Polytetrafluoroethylene has good wear resistance and chemical stability, and the formation of a coating can improve the wear resistance, breaking strength and tensile strength of the fiber.
[0047] S4: Spinning the hollow polyimide composite fiber to obtain polyimide yarn, and weaving the polyimide yarn as warp yarn and the polyvinyl alcohol yarn as weft yarn to obtain a multifunctional fiber composite fabric.
[0048] The fineness of polyimide yarn in S4 is 40-60D, the fineness of polyvinyl alcohol yarn is 30-50D, the fiber counts of polyimide yarn and polyvinyl alcohol yarn are 20-30F and 15-20F respectively, and the warp and weft densities of the multifunctional fiber composite fabric are 40-50 strands / cm and 55-60 strands / cm respectively. The fineness of polyimide yarn is higher, which can provide higher strength and wear resistance, and is suitable as the warp yarn of the fabric. The fineness of polyimide yarn is lower and has better softness, which helps to improve the comfort and fit of the fabric. The combination of the high strength of polyimide yarn and the softness of polyvinyl alcohol yarn can improve the tensile and compression resistance of the fabric.
[0049] S5: The multifunctional fiber composite fabric is combined with the outer layer of the jacket to obtain a multifunctional fiber composite fabric jacket.
[0050] The multifunctional fiber composite fabric in S5 is combined with the outer layer of the jacket by sewing or bonding. The outer layer of the jacket includes: a jacket body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket.
[0051] Cellulose and polyimide are made into coaxial fibers, and the coaxial fibers are subjected to ultrasonic treatment and alkali treatment in succession, and nylon 66 is sprayed on the fiber surface. The obtained fibers are spun and woven, and made into a jacket, so that polyimide and nylon 66 can form coaxial fiber hollow fibers, and polyimide can form a hollow structure while being tightly combined with nylon 66, while improving the thermal insulation performance and mechanical properties of the multifunctional fiber, enhancing the thermal insulation performance and mechanical properties of the jacket, and solving the defects of insufficient thermal insulation performance and mechanical properties of the jacket in the prior art. Embodiment 1
[0052] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0053] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0054] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 20 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:2 to obtain a hollow polyimide fiber.
[0055] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0056] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0057] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 2
[0058] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0059] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0060] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 30 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:2 to obtain a hollow polyimide fiber.
[0061] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0062] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0063] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 3
[0064] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0065] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0066] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:2 to obtain a hollow polyimide fiber.
[0067] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0068] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0069] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 4
[0070] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0071] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0072] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 50 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:2 to obtain a hollow polyimide fiber.
[0073] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0074] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0075] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 5
[0076] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0077] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0078] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 60 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:2 to obtain a hollow polyimide fiber.
[0079] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0080] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0081] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 6
[0082] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0083] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0084] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:1.5 to obtain a hollow polyimide fiber.
[0085] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0086] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0087] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 7
[0088] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0089] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0090] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:3 to obtain a hollow polyimide fiber.
[0091] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0092] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0093] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 8
[0094] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0095] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0096] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 min. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:4 to obtain a hollow polyimide fiber.
[0097] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0098] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0099] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 9
[0100] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0101] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0102] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 min. During the soaking process of the alkaline solution, the original polyimide fiber was stretched with a stretching ratio of 1:4.5 to obtain a hollow polyimide fiber.
[0103] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0104] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0105] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 10
[0106] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0107] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0108] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:3 to obtain a hollow polyimide fiber.
[0109] S3: spraying a 10% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0110] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0111] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 11
[0112] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0113] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0114] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:3 to obtain a hollow polyimide fiber.
[0115] S3: spraying a 20% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0116] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0117] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket. Embodiment 12
[0118] This embodiment provides a jacket made of a multifunctional fiber composite fabric, and the preparation method is as follows:
[0119] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0120] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:3 to obtain a hollow polyimide fiber.
[0121] S3: spraying a nylon 66 solution with a mass fraction of 25% onto the surface of the hollow polyimide fiber for 20 minutes, and then immersing the hollow polyimide fiber in a polytetrafluoroethylene solution with a mass fraction of 20% for 0.5 hours to obtain a hollow polyimide composite fiber;
[0122] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0123] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, so as to obtain a multifunctional fiber composite fabric jacket.
[0124] Comparative Example 1
[0125] This comparative example provides a jacket, and the preparation method is as follows:
[0126] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0127] S2: soaking the original polyimide fiber in a 10% sodium hydroxide solution for 1 hour, and stretching the original polyimide fiber during the soaking process, with a stretching ratio of 1:3, to obtain a hollow polyimide fiber;
[0128] S3: spraying a 20% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0129] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0130] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, thereby obtaining a jacket.
[0131] Comparative Example 2
[0132] This embodiment provides a jacket, and the preparation method is as follows:
[0133] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0134] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 min to obtain a hollow polyimide fiber.
[0135] S3: spraying a 15% by mass nylon 66 solution onto the surface of the hollow polyimide fiber for 20 min, and then immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0136] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0137] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, thereby obtaining a jacket.
[0138] Comparative Example 3
[0139] This embodiment provides a jacket, and the preparation method is as follows:
[0140] S1: Spinning cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, with cellulose as the core fiber and polyimide as the outer fiber, the mass fraction of cellulose in the cellulose spinning solution is 40%, the mass fraction of polyimide in the polyimide spinning solution is 30%, the extrusion speed of the cellulose spinning solution is 8 ml / min, the extrusion speed of the polyimide spinning solution is 4 ml / min, the diameter of the core fiber is 8 μm, and the outer diameter of the outer fiber is 16 μm, to obtain the original polyimide fiber;
[0141] S2: The original polyimide fiber was treated with ultrasound and then immersed in a 10% sodium hydroxide solution for 1 hour. The frequency of the ultrasound treatment was 40 Hz and the treatment time was 40 minutes. During the soaking process of the alkaline solution, the original polyimide fiber was stretched at a stretching ratio of 1:3 to obtain a hollow polyimide fiber.
[0142] S3: immersing the hollow polyimide fiber in a 20% by mass polytetrafluoroethylene solution for 0.5 h to obtain a hollow polyimide composite fiber;
[0143] S4: spinning the hollow polyimide composite fiber to obtain a polyimide yarn, using the polyimide yarn as the warp yarn and the polyvinyl alcohol yarn as the weft yarn for weaving, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, to obtain a multifunctional fiber composite fabric;
[0144] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, thereby obtaining a jacket.
[0145] Comparative Example 4
[0146] This embodiment provides a jacket, and the preparation method is as follows:
[0147] S1: Spinning polyimide fiber to obtain polyimide yarn, weaving the polyimide yarn as warp yarn and polyvinyl alcohol yarn as weft yarn, the fineness of the polyimide yarn is 50D, the fineness of the polyvinyl alcohol yarn is 40D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 30F and 20F respectively, the warp and weft densities of the multifunctional fiber composite fabric are 45 strands / cm and 55 strands / cm respectively, and obtaining a multifunctional fiber composite fabric;
[0148] S5: The multifunctional fiber composite fabric is sewn and combined with the outer layer of the jacket, wherein the outer layer of the jacket comprises: a body, a hood and a zipper, and the multifunctional fiber composite fabric is arranged on the inner side of the outer layer of the jacket, thereby obtaining a jacket.
[0149] Samples of the jackets in Examples 1 to 12 and Comparative Examples 1 to 4 were taken, and the warmth retention was tested according to the standard GB / T11048-2008 and the fabric strength was tested by a strength tester, and tensile force was applied to the warp and weft directions of the fabric until it broke. The obtained data results are shown in Table 1:
[0150] Table 1 Crowe value and breaking strength test data of Examples 1 to 12 and Comparative Examples 1 to 4
[0151]
[0152] It can be seen from Table 1 that the Crowe values and breaking strengths in Examples 1 to 12 are greater than those in Comparative Examples 1 to 4, and the Crowe values and breaking strengths are positively correlated with the warmth retention and mechanical properties of the jacket, respectively. The method for preparing a jacket made of a multifunctional fiber composite fabric in the present application is superior.
[0153] In Examples 1 to 5, as the frequency of ultrasonic treatment gradually increases, the Crowe value and breaking strength of the sample first increase and then decrease. Ultrasonic treatment causes the fiber surface to be subjected to force more evenly, thereby improving the surface activity and bonding properties of the fiber, making the bonding between the fibers stronger, thereby improving the breaking strength of the fabric. Ultrasonic treatment optimizes the pore structure and improves the thermal insulation performance of the fabric. However, if the frequency of ultrasonic treatment is too high, it will cause excessive damage to the fiber and destruction of the pore structure, thereby reducing its warmth retention and breaking strength. The preferred embodiment is Example 3.
[0154] In Example 3 and Examples 6 to 9, as the fiber stretching ratio gradually increases, the Crowe value and breaking strength of the sample first increase and then decrease. Stretching can improve the orientation of the fiber molecular chain, increase the crystallinity and intermolecular force of the fiber, thereby improving the breaking strength. The porosity can be increased during the stretching process, and the thermal insulation performance of the fiber can be enhanced. An excessively high stretching ratio may lead to excessive orientation of the internal structure of the fiber, and even cause molecular chain breakage or excessive stretching damage, which will reduce the breaking strength of the fiber, and destroy the pore structure of the fiber, reducing its thermal insulation properties. The preferred embodiment is Example 7.
[0155] In Example 7 and Examples 10 to 12, as the concentration of nylon 66 solution increases, the Crowe value and breaking strength of the samples first increase and then decrease. This is because nylon 66 has good mechanical properties and thermal insulation properties. An appropriate concentration can form a uniform and continuous coating, thereby improving the breaking strength and thermal insulation properties of the fiber. However, when the concentration is too high, the coating becomes too thick, which affects the flexibility and air permeability of the fiber, and affects its thermal insulation properties and wearing comfort. The fiber becomes more brittle after coating, resulting in a decrease in breaking strength. The best embodiment is Example 11.
[0156] Compared with Example 11, Comparative Examples 1 to 3 lack ultrasonic treatment, fiber stretching and adding nylon 66 coating on the outside of the hollow polyimide fiber, respectively. The Crom values and breaking strengths of Comparative Examples 1 to 3 are less than those of Example 11, and the Crom values and breaking strengths of Comparative Examples 1 to 3 are greater than those of Comparative Example 4. The preparation method of the jacket in the present application is superior.
[0157] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a jacket made of a multifunctional fiber composite fabric, characterized in that: The following steps are involved: S1: Coaxial spinning is performed using cellulose as a core fiber and polyimide as an outer fiber to obtain an original polyimide fiber, wherein the coaxial spinning method is to spin cellulose spinning solution and polyimide spinning solution using a coaxial spinning device, the extrusion speed of the cellulose spinning solution is 7-9 ml / min, the extrusion speed of the polyimide spinning solution is 3-5 ml / min, the diameter of the core fiber is 4-8 μm, and the outer diameter of the outer fiber is 12-16 μm; S2: treating the original polyimide fiber with ultrasound and then immersing it in an alkaline solution to obtain a hollow polyimide fiber, wherein the frequency of the ultrasound treatment in S2 is 30-50 Hz, the treatment time is 20-40 min, the main component of the alkaline solution is sodium hydroxide, the concentration of the alkaline solution is 10-20%, and the immersion time is 1-1.5 h; S3: spraying nylon 66 solution onto the surface of the hollow polyimide fiber to obtain a hollow polyimide composite fiber; S4: spinning the hollow polyimide composite fiber to obtain polyimide yarn, and weaving the polyimide yarn as warp yarn and polyvinyl alcohol yarn as weft yarn to obtain a multifunctional fiber composite fabric; S5: combining the multifunctional fiber composite fabric with the outer layer of the jacket to obtain a jacket made of multifunctional fiber composite fabric.
2. The method for preparing a jacket made of a multifunctional fiber composite fabric according to claim 1, characterized in that: The mass fraction of the solvent in the cellulose spinning solution is 55-65%, and the solvent is ethanol, and the mass fraction of ethanol is 85-95%. The mass fraction of polyimide in the polyimide spinning solution is 20%-30%, and the solvent is N,N-dimethylacetamide.
3. The method for preparing a jacket made of a multifunctional fiber composite fabric according to claim 1, characterized in that: In S2, the fiber is stretched during the soaking in the alkaline solution, the stretching ratio is 1:2-4, and the stretching direction is along the fiber axis.
4. The method for preparing a jacket made of a multifunctional fiber composite fabric according to claim 1, characterized in that: The nylon 66 solution in S3 contains: nylon 66, formic acid and adhesive, the mass ratio of the nylon 66, the formic acid and the adhesive is: 15-20:70-85:1-2, and the spraying time is 20-30 minutes.
5. The method for preparing a jacket made of a multifunctional fiber composite fabric according to claim 1, characterized in that: In S3, after spraying nylon 66 solution on the surface of the hollow polyimide fiber to form a nylon 66 fiber layer, the hollow polyimide fiber is immersed in a polytetrafluoroethylene solution for 0.5-1h, and the mass fraction of the polytetrafluoroethylene is 20-30%.
6. The method for preparing a jacket made of a multifunctional fiber composite fabric according to claim 1, characterized in that: The fineness of the polyimide yarn in S4 is 40-60D, the fineness of the polyvinyl alcohol yarn is 30-50D, the fiber numbers of the polyimide yarn and the polyvinyl alcohol yarn are 20-30F and 15-20F respectively, and the warp and weft densities of the multifunctional fiber composite fabric are 40-50 strands / cm and 55-60 strands / cm respectively.
7. The method for preparing a jacket made of a multifunctional fiber composite fabric according to claim 1, characterized in that: The multifunctional fiber composite fabric in S5 is combined with the outer layer of the jacket by sewing or bonding.
Citation Information
Patent Citations
Method for producing composite hollow nanofiber filter core
CN106975363A
Polyimide modified nylon composition and preparation method
CN109082112A
Polyester / nylon composite material as well as preparation method and application thereof
CN113773508A
Composite diaphragm for hydrogen production by alkaline electrolyzed water and preparation method of composite diaphragm
CN116219492A
Three-dimensional fireproof quick-dry velvet fabric with inclined grids
CN217145193U