A high-strength, water-resistant, flame-retardant artificial stone board imitating fossil wood and its preparation method and application
Through the sol-gel method, the problem of weak and flammable bonding of inorganic artificial board interfaces was solved, and high-strength, water-resistant, flame-retardant, artificial stone slabs of imitation wood fossils were prepared, achieving environmental protection, Economical application of building materials.
Patent Information
- Application Number
- CN202411181689.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing inorganic artificial boards have weak bonding between wood particles and inorganic components, resulting in low mechanical strength, flammable and high production costs. The use of a traditional artificial board with aldehyde adhesive will release formaldehyde gas, causing environmental pollution.
The sol-gel method is used to imitate the natural petrochemical process. The silicate sol configured with ethyl orthosilicate, ethanol and aqueous solution reacts with wood particles to realize the penetration and gelation of petrochemical agents in and between wood particles, forming high strength. , water-resistant, flame-retardant imitation wood fossil artificial stone slab.
Prepare artificial stone slabs with imitation wood fossils with high mechanical strength, good flame retardancy and good water resistance, which reduces production costs, avoids the release of formaldehyde gas, meets the needs of high-quality imitation wood fossil materials, and provides environmentally friendly building materials choose.
Smart Images

Figure CN118700280B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of building functional materials, and more specifically to a high-strength, water-resistant, flame-retardant wood fossil-like artificial stone board and a preparation method and application thereof. Background Art
[0002] Fossilized wood is a kind of wood fossil that exists in nature. Over billions of years, with the gradual degradation of wood components and the slow penetration of silicon sources, some wood components were eventually replaced by silica, but the original wood cell structure was still maintained. Fossilized wood not only has the friendly appearance of natural wood, but also has the excellent weather resistance of stone. It can preserve the microscopic and macroscopic morphology of wood from billions of years ago. The exquisite reproduction process in fossilized wood is due to the affinity of the hydroxyl groups of cellulose in wood and the silica in the earth's crust, and it also proves the feasibility of forming a close bond between silica and wood. However, natural fossilized wood resources are scarce, and the mining and processing process is time-consuming and labor-intensive, has a great impact on the environment, and is also extremely expensive. Therefore, the market has an urgent need for materials that can replace natural fossilized wood.
[0003] A large amount of waste wood particles will be generated during the wood processing process, which will not only cause waste but also pollute the environment. The reuse of waste wood particles can improve the utilization efficiency of resources, reduce environmental pollution and reduce production costs. Converting waste wood particles into high value-added products can greatly improve economic benefits and conform to the concept of sustainable development. In the industrial production process, the recycling of waste wood particles is often made into artificial wood boards under high temperature and high pressure. However, traditional artificial wood boards are extremely flammable and have fire hazards, and their preparation generally relies on formaldehyde-containing adhesives, which release a large amount of formaldehyde gas during production and use, causing environmental pollution and endangering health.
[0004] Inorganic artificial boards such as gypsum, silicate cement, magnesia cement, and aluminum phosphate have appeared one after another, but the current inorganic components can only be filled between wood particles, which makes the inorganic components and the interface of wood particles extremely weak, becoming an important problem restricting their development. The inorganic component precursors have poor permeability between wood particles and often only rely on mechanical intercalation with some pores on the surface of the wood, which makes their mechanical strength low and easily reacts, dissolves or expands to cause damage when exposed to water. The artificial boards prepared in this way are prone to poor water stability, poor strength, and long preparation time. At the same time, the hot pressing process in the manufacturing process relies on large hot pressing equipment, which greatly increases the production cost. Summary of the invention
[0005] In order to solve the above problems, the first purpose of the present invention is to provide a method for preparing a high-strength, water-resistant and flame-retardant imitation wood fossil artificial stone board. The present invention is inspired by the formation process of wood fossils. By imitating the physical penetration and chemical reaction pathways in the process, the hydrophilicity of the wood cell wall is regulated, and the sol-gel method is used to achieve good penetration and gelation of the petrochemical agent silica sol in and between wood particles, and to achieve a close combination between the wood and silica interface. Finally, a wood fossil imitation artificial stone board with high mechanical strength, good flame retardancy and good water resistance is prepared, which not only fills the market demand for high-quality wood fossil imitation materials, but also provides a new idea for the reuse of waste wood particles, and also provides an environmentally friendly and economical choice for the construction and decoration industries, with broad application prospects.
[0006] The second object of the present invention is to provide a high-strength, water-resistant and flame-retardant imitation wood fossil artificial stone board.
[0007] The third object of the present invention is to provide an application of a wood fossil imitation artificial stone board in the preparation of flame retardant and fireproof building materials.
[0008] The petrification agent of the present invention is a silica sol prepared from ethyl orthosilicate, ethanol and aqueous solution, and is a chemical substance used to imitate the natural petrification process. By reacting with wood, the wood is hardened and obtains a microstructure and physical properties similar to natural petrified wood. Petrification treatment refers to the process in which wood reacts chemically with the petrification agent and gradually petrifies. In the process, inorganic substances are gradually deposited, and finally a material similar to a natural fossil or petrified wood is formed. The petrification reaction simulates the effect of wood petrification in the natural environment.
[0009] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0010] The invention discloses a method for preparing a high-strength, water-resistant and flame-retardant artificial stone board imitating wood fossils, wherein the artificial stone board imitating wood fossils is prepared by using a petrifying agent silica sol to penetrate and gelate in and between wood particles for many times;
[0011] 1) Stirring the pretreated wood particles and petrochemical agent, placing the mixture in a mold after uniform mixing, and drying in an oven to obtain an artificial stone slab;
[0012] 2) The artificial stone slab is completely immersed in the petrochemical agent for 20-40 minutes under a vacuum degree of 1-5 Pa, and then taken out and placed in an oven for drying;
[0013] 3) Repeat the impregnation-drying operation of step 2) for more than 3 times, so that the petrification agent fully penetrates into and between the wood particles, and gels and grows silica multiple times inside the artificial stone board, and finally obtains the imitation wood fossil artificial stone board;
[0014] wherein, by volume percentage, the petrochemical agent is composed of 30-60% of ethyl orthosilicate, 10-30% of anhydrous ethanol and 30-50% of water; or
[0015] The petrochemical agent is composed of 10-20% of tetraethyl orthosilicate, 40-60% of anhydrous ethanol and 30-40% of water; or
[0016] The petrochemical agent consists of 20-80% of ethyl orthosilicate and 20-80% of water.
[0017] Different from the poor fluidity of common inorganic components and poor ability to bind to the wood interface, which leads to low mechanical strength of artificial stone slabs, the present invention uses the sol-gel method to make the petrification agent exist in the form of small molecular silicate with good fluidity in step 1 and step 2, which is conducive to good penetration and close combination in the pretreated wood particles and between wood particles. In the drying and curing stage, the petrification agent with good fluidity undergoes in-situ polymerization inside the artificial stone slab, and its fluidity gradually weakens and finally condenses in-situ to form silica, which plays a petrifying role. Since wood particles are mostly cellulose and hemicellulose, their surfaces have a large number of hydroxyl groups. When the sol-gel process occurs, the hydroxyl groups of silicate can easily form hydrogen bonds with the hydroxyl groups on the surface of wood. The rich hydrogen bonds greatly improve the binding ability of the interface between wood and silica, and new silicate can also continue to condense on the surface of the already gelled silica. Just as when the wood fossil is formed, the groundwater in the soil where the wood is located constantly rises and falls. In the cycle of impregnation-drying, the present invention uses the sol-gel method to continuously grow silica in the wood particles and between the wood particles to achieve a gradual increase in the strength of the artificial stone slab imitating the wood fossil.
[0018] Furthermore, in step 1), 600-800 ml of petrochemical agent is added to every 100 g of wood particles for mixing.
[0019] Furthermore, in step 1), 750 ml of petrochemical agent is added per 100 g of wood particles for mixing.
[0020] The present invention screens the raw material ratio for the sol-gel method, and studies have found that when wood is in contact with a petrochemical agent, bulk polymerization between the bulk solution and the interface polymerization with the wood form a competitive relationship. When the wood has a strong affinity with the petrochemical agent, the petrochemical agent not only polymerizes in the wood pores but also penetrates and polymerizes in the wood cell wall to achieve close bonding, otherwise it may only polymerize in the bulk phase in the wood pores. The raw material ratio based on the appropriate sol-gel method solves the problem of weak interface bonding between the petrochemical agent and the wood.
[0021] Further, in step 3), the impregnation-drying operation of step 2) is repeated 8-15 times to finally obtain the imitation wood fossil artificial stone board. The number of impregnation-drying mainly affects the mass proportion of silica in the imitation wood fossil artificial stone board. When the amount of petrifying agent used in the impregnation is constant, the higher the number of impregnation-drying, the greater the proportion of silica in the obtained imitation wood fossil artificial stone board. If the number of impregnation-drying is too many, although the proportion of silica can be increased, since silica may have been fully filled in and between the wood particles, further increasing the proportion of silica at this time will only cause silica to accumulate on the surface of the imitation wood fossil artificial stone board, which not only wastes raw materials, but also affects the mechanical properties of the product. Therefore, the number of impregnation-drying should not exceed 15 times. Technicians can use the amount of petrifying agent used in the impregnation to adjust the silica proportion requirement under a limited number of impregnation-drying times.
[0022] Furthermore, oven drying is to promote gelation of the petrochemical agent within and between wood particles, and the drying temperature of the oven is 20-60°C.
[0023] Further, the mass proportion of silicon dioxide in the imitation wood fossil artificial stone board is 40-70wt%, preferably 53-70wt%, and more preferably 65-70%; illustratively, the mass proportion of silicon dioxide in the imitation wood fossil artificial stone board can be 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, etc.
[0024] Furthermore, the petrochemical agent is composed of 30-50% of ethyl orthosilicate, 10-30% of anhydrous ethanol and 30-50% of water, or the petrochemical agent is composed of 20-80% of ethyl orthosilicate and 20-80% of water, by volume percentage. Within this formula range, in step 3), the dipping-drying operation of step 2) is repeated for more than 3 times, preferably 8-15 times, which can ensure good penetration and close bonding of the petrochemical agent in and between wood particles, and also make the mass proportion of silicon dioxide in the imitation wood fossil artificial stone board within a reasonable control range, so that there will not be too much silicon dioxide accumulated on the surface of the imitation wood fossil artificial stone board, affecting its mechanical properties.
[0025] Furthermore, the selected wood particles can be waste wood particles generated during wood processing, and the source of the waste wood particles is not limited. Preferably, the particle size of the wood particles is 40-60 meshes.
[0026] In order to increase the hydrophilic cellulose content in the cell wall of wood particles, increase the functional groups that can be bound by petrochemical agents, and reduce the hydrophobic lignin content, the wood particles should be pretreated to adjust the hydrophilic and hydrophobic properties of the wood surface and cell wall, so that it becomes more hydrophilic, easy to penetrate, and easier to bind tightly with petrochemical agents. The specific steps of the pretreatment operation are as follows:
[0027] Boil the wood particles in a mixed solution of NaOH and Na2SO3 for 8-12 hours, and then rinse the wood particles with water until they are neutral.
[0028] Furthermore, in the mixed solution, the concentration of NaOH is 1.5-2.5 mol / L, and the concentration of Na2SO3 is 0.2-0.6 mol / L.
[0029] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0030] The invention discloses a high-strength, water-resistant and flame-retardant wood-like fossil artificial stone board prepared by the preparation method as described above.
[0031] In order to achieve the third object, the present invention adopts the following technical solutions:
[0032] The invention discloses an application of the above-mentioned imitation wood fossil artificial stone board in preparing flame retardant and fireproof building materials.
[0033] The beneficial effects of the present invention are as follows:
[0034] The present invention provides a method for preparing a high-strength, water-resistant and flame-retardant artificial stone board imitating wood fossils. The preparation method imitates the formation process of wood fossils and uses a sol-gel method to make a petrifying agent and wood closely combined for preparation. The petrifying agent has good fluidity and can ensure that the silicon source fully penetrates into and between wood particles during multiple petrification processes. When drying, the petrifying agent polymerizes into silicon dioxide in situ inside and between wood particles. After multiple impregnation-drying cycles, the preparation of the artificial stone board imitating wood fossils is completed. In order to make the petrifying agent penetrate better and make the wood and silicon dioxide closely combined, the wood particles are pretreated in advance, thereby adjusting the hydrophilic and hydrophobic properties of the wood surface to make it more hydrophilic.
[0035] The preparation method of the invention is simple to operate, does not require hot pressing and curing operations, can complete the preparation within 100 hours under normal pressure, has high preparation efficiency, low cost, and is environmentally friendly.
[0036] The weight ratio of silicon dioxide in the imitation wood fossil artificial stone board obtained by the present invention is 40-70wt%, and the mechanical strength of the imitation wood fossil artificial stone board is 14.72-24.78 MPa, which is equal to or higher than the bending strength of common building stones or cement, such as granite, marble, limestone, sandstone, etc., and can better meet the strength, weather resistance, and formaldehyde-free emission requirements of actual building materials. Taking the scheme of Example 3 as an example, the thickness expansion rate of the imitation wood fossil artificial stone board of the present invention after immersion in water for 24 hours is less than 1%, and it has good immersion dimensional stability. 2 Under the thermal radiation power, the flame retardant ignition time can reach 93 seconds, and the total heat release rate is 7.84 MJ / m 2 81% lower than natural wood, average carbon monoxide release 0.016 kg / kg, 47% lower than natural wood, average carbon dioxide release 0.84 kg / kg, 33% lower than natural wood, total smoke release 0.16 m 2 / m 2 Compared with natural wood, it is 93% lower, and the flame retardant properties of imitation wood fossil artificial stone board are excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0038] Figure 1A The electron microscope and EDS images of Scheme 3 in the early exploration are shown.
[0039] Figure 1B The electron microscope and EDS images of Scheme 14 in the early exploration are shown.
[0040] Figure 2A A photograph showing the burning of natural wood in Test Example 3 is shown.
[0041] Figure 2B A photograph showing the burning of the fossil wood-like artificial stone board of Example 3 in Test Example 3. DETAILED DESCRIPTION
[0042] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0043] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0044] Early exploration
[0045] First, the penetration effect of different petrochemical agent formulations on wood particles was investigated.
[0046] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0047] 2) Tetraethyl orthosilicate (TEOS), anhydrous ethanol (EtOH) and water are prepared according to the volume percentages in Table 1 to obtain a petrochemical agent.
[0048] 3) The pretreated wood particles are stirred with each petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60°C for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of wood particles and petrochemical agents is such that 750 ml of petrochemical agent is added to every 100 g of wood particles.
[0049] 4) The artificial stone slab was completely immersed in the petrification agent of the same formula, immersed for 30 minutes under a vacuum degree of 1-5 Pa, and then placed in a 60°C oven for drying for 4 hours to complete a petrification treatment to obtain an artificial stone slab imitating fossil wood. The microscopic conditions of different artificial stone slabs imitating fossil wood were observed using an electron microscope and EDS.
[0050] Table 1
[0051]
[0052] Note: The criterion for good penetration is whether the petrochemical agent polymerizes into silica in situ within the cell walls of the wood particles.
[0053] Table 1 lists some of the formulations explored during the research process. Combined with electron microscopy and EDS, it can be clearly observed that the petrochemical agents in schemes 1-10 can penetrate well into the wood particles, the petrochemical agents can penetrate into the wood cell walls, and the silica forms a tight bond with the wood interface. However, schemes 11-16 cannot achieve good penetration into the wood particles, and the silica is mainly filled in the wood pores, indicating that the mass ratio of ethyl orthosilicate, anhydrous ethanol and water can be used to adjust the penetration of petrochemical agents into wood particles.
[0054] In order to better illustrate the above situation, the electron microscope and EDS images of Scheme 3 and Scheme 14 are provided as examples for detailed explanation. Figure 1A and Figure 1B , Figure 1AFrom left to right in the figure are the photograph of the artificial stone board imitating fossil wood obtained in Scheme 3 under a scanning electron microscope at 2000 times magnification and the scanning image of the silicon element distribution by an energy dispersive spectrometer. It is found that the silicon dioxide in the artificial stone board imitating fossil wood obtained in Scheme 3 is clearly and evenly distributed inside the cell wall, indicating that the petrifying agent with good permeability to wood particles is conducive to the uniform distribution and tight combination of silicon dioxide inside the cell wall after gelation, which is beneficial to the improvement of the mechanical properties, fire resistance and water resistance of the material. Figure 1B From left to right in the figure are the 2000 times magnified scanning electron microscope photo of the artificial stone plate imitating fossil wood obtained in Scheme 14 and the scanning image of the silicon element distribution by the energy spectrometer. In the artificial stone plate imitating fossil wood obtained in Scheme 14, silicon dioxide is not visible in the cell wall and is mainly distributed in the pores.
[0055] The present invention exemplarily demonstrates some typical experimental results within the range of petrochemical agent formula (i.e., by volume percentage, the petrochemical agent consists of 30-60% of tetraethyl orthosilicate, 10-30% of anhydrous ethanol and 30-50% of water; or the petrochemical agent consists of 10-20% of tetraethyl orthosilicate, 40-60% of anhydrous ethanol and 30-40% of water; or the petrochemical agent consists of 20-80% of tetraethyl orthosilicate and 20-80% of water), indicating that it is beneficial to improve the mechanical properties, water resistance and fire resistance of the imitation wood fossil artificial stone board while obtaining a good penetration effect.
[0056] In order to better demonstrate the mechanical properties, water resistance and fire resistance of the imitation wood fossil artificial stone board, the formula of Scheme 3 is used as an example for subsequent research. It can be understood by technicians that when the other formulas with good penetration effects in Table 1 are used to prepare the imitation wood fossil artificial stone board, the mechanical properties, water resistance and fire resistance results are not significantly different from those of the imitation wood fossil artificial stone board obtained in Scheme 3.
[0057] Example 1
[0058] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0059] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 40% of tetraethyl orthosilicate, 30% of anhydrous ethanol and 30% of water (all by volume) to obtain a petrochemical agent.
[0060] 3) The pretreated wood particles and the petrochemical agent are stirred and placed in a polytetrafluoroethylene mold after being mixed evenly, and dried in an oven at 60° C. for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of the wood particles.
[0061] 4) The artificial stone slab is completely immersed in the petrification agent at a vacuum degree of 1-5 Pa for 30 minutes. After being taken out, it is placed in a 60°C oven to dry for 4 hours to complete the petrification treatment.
[0062] 5) Repeating the petrification process three more times according to step 4), preparing a fossilized wood artificial stone board by repeated vacuum impregnation-drying. According to the test, in the prepared fossilized wood artificial stone board, the mass proportion of silicon dioxide in the fossilized wood artificial stone board is 53wt%.
[0063] Example 2
[0064] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0065] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 40% of tetraethyl orthosilicate, 30% of anhydrous ethanol and 30% of water (all by volume) to obtain a petrochemical agent.
[0066] 3) The pretreated wood particles are stirred with the petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60° C. for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of the wood particles.
[0067] 4) The artificial stone slab is completely immersed in the petrification agent at a vacuum degree of 1-5 Pa for 30 minutes. After being taken out, it is placed in a 60°C oven to dry for 4 hours to complete the petrification treatment.
[0068] 5) Repeating the petrification process 8 more times according to step 4), preparing a fossilized wood artificial stone board by repeated vacuum impregnation-drying. According to the test, in the prepared fossilized wood artificial stone board, the mass proportion of silicon dioxide in the fossilized wood artificial stone board is 67wt%.
[0069] Example 3
[0070] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0071] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 40% of tetraethyl orthosilicate, 30% of anhydrous ethanol and 30% of water (all by volume) to obtain a petrochemical agent.
[0072] 3) The pretreated wood particles are stirred with the petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60° C. for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of the wood particles.
[0073] 4) The artificial stone slab is completely immersed in the petrification agent at a vacuum degree of 1-5 Pa for 30 minutes. After being taken out, it is placed in a 60°C oven to dry for 4 hours to complete the petrification treatment.
[0074] 5) Repeating the petrification process 13 times according to step 4) to prepare a fossilized wood artificial stone board by repeated vacuum impregnation-drying. According to the test, the prepared fossilized wood artificial stone board has a silicon dioxide content of 70wt% of the fossilized wood artificial stone board.
[0075] Comparative Example 1
[0076] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0077] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 40% of tetraethyl orthosilicate, 30% of anhydrous ethanol and 30% of water (all by volume) to obtain a petrochemical agent.
[0078] 3) The pretreated wood particles are stirred with the petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60°C for 4 hours to promote the gelation process, completing a petrochemical treatment to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of wood particles to obtain the artificial stone slab.
[0079] According to the test, in the prepared imitation wood fossil artificial stone board, the mass proportion of silicon dioxide in the imitation wood fossil artificial stone board is 28wt%.
[0080] Comparative Example 2
[0081] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0082] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 40% of tetraethyl orthosilicate, 50% of anhydrous ethanol and 10% of water (all by volume) to obtain a petrochemical agent.
[0083] 3) The pretreated wood particles are stirred with the petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60° C. for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of the wood particles.
[0084] 4) The artificial stone slab is completely immersed in the petrification agent at a vacuum degree of 1-5 Pa for 30 minutes. After being taken out, it is placed in a 60°C oven to dry for 4 hours to complete the petrification treatment.
[0085] 5) Repeating the petrification process 13 times according to step 4) to prepare a fossilized wood artificial stone board by repeated vacuum impregnation-drying. According to the test, the weight of silicon dioxide in the prepared fossilized wood artificial stone board is 58wt%.
[0086] Comparative Example 3
[0087] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0088] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 60% of tetraethyl orthosilicate, 10% of anhydrous ethanol and 30% of water (all by volume) to obtain a petrochemical agent.
[0089] 3) The pretreated wood particles are stirred with the petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60° C. for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of the wood particles.
[0090] 4) The artificial stone slab is completely immersed in the petrification agent at a vacuum degree of 1-5 Pa for 30 minutes. After being taken out, it is placed in a 60°C oven to dry for 4 hours to complete the petrification treatment.
[0091] 5) Repeating the petrification process 8 more times according to step 4), preparing a fossilized wood artificial stone board by repeated vacuum impregnation-drying. According to the test, in the prepared fossilized wood artificial stone board, the mass proportion of silicon dioxide in the fossilized wood artificial stone board is 70wt%.
[0092] Comparative Example 4
[0093] 1) 138.97 g of waste basswood wood particles were sieved to 40-60 mesh, boiled in a mixed solution containing 2 mol / L NaOH and 0.4 mol / L Na2SO3 for 10 h, and then washed with running water until the wood particles were neutral to obtain pretreated wood particles.
[0094] 2) Tetraethyl orthosilicate, anhydrous ethanol and water are prepared according to 20% of tetraethyl orthosilicate, 40% of anhydrous ethanol and 40% of water (all by volume) to obtain a petrochemical agent.
[0095] 3) The pretreated wood particles are stirred with the petrochemical agent, and after being evenly mixed, they are placed in a polytetrafluoroethylene mold and dried in an oven at 60° C. for 4 hours to promote the gelation process to obtain an artificial stone slab, wherein the amount of the wood particles and the petrochemical agent is such that 750 ml of the petrochemical agent is added to every 100 g of the wood particles.
[0096] 4) The artificial stone slab is completely immersed in the petrification agent at a vacuum degree of 1-5 Pa for 30 minutes. After being taken out, it is placed in a 60°C oven to dry for 4 hours to complete the petrification treatment.
[0097] 5) Repeating the petrification process 23 times according to step 4) to prepare a fossilized wood artificial stone board by repeated vacuum impregnation-drying. According to the test, the prepared fossilized wood artificial stone board has a silicon dioxide content of 70wt% of the fossilized wood artificial stone board.
[0098] Test Example 1 Mechanical Properties
[0099] The static bending strength test was carried out in accordance with GB / T 35160.2-2017 “Test methods for synthetic stone Part 2: Determination of flexural strength”. The results are shown in Table 2.
[0100] Table 2
[0101]
[0102] By comparing Examples 1-3 and Comparative Example 1, it is known that the number of petrochemical treatments will affect the flexural strength. Examples 1-3 are equal to or higher than the flexural strength (3-20 MPa) of common building stones or cement, such as granite, marble, limestone, sandstone, etc. Under this preparation condition, the flexural strength reaches the maximum when the petrochemical treatment is repeated 15 times, which is 24.78±1.40 (MPa).
[0103] By comparing Example 3 with Comparative Example 2, it is known that the imitation wood fossil artificial stone board without good penetration effect has lower bending strength than the imitation wood fossil artificial stone board with good penetration effect, indicating that good permeability will affect the bonding condition of the petrifying agent and wood interface and further affect the mechanical strength of the material.
[0104] In Comparative Example 3, since the content of ethyl orthosilicate in the petrochemical agent is too high, the amount of petrochemical treatment is too much, which will increase the amount of silica on the surface of the artificial stone slab and reduce the static bending strength. Therefore, a more preferred solution is to control the volume proportion of ethyl orthosilicate in the petrochemical agent to less than 50%.
[0105] In Comparative Example 4, since the content of ethyl orthosilicate in the petrochemical agent is relatively low, the amount of petrochemical treatment is too small, and the silica is more likely to produce tiny defects after gel condensation, which is not conducive to maintaining the mechanical strength of the imitation wood fossil artificial stone slab. Therefore, a more preferred solution is to control the volume proportion of ethyl orthosilicate in the petrochemical agent to more than 30%.
[0106] Test Example 2 Water resistance
[0107] The thickness expansion rate test method is to take five samples prepared in Example 3, use a vernier caliper to measure their thickness three times, and take the average value, completely immerse them in deionized water for 24 hours, take them out, and immediately measure their thickness again. Calculate according to the following formula: thickness expansion rate = (thickness after immersion in water - thickness before immersion in water) / thickness before immersion in water x 100%. The results are shown in Table 3. It can be seen from Table 3 that the imitation wood fossil artificial stone board prepared by the present invention has strong water immersion stability without adding functional components, which is inseparable from the good penetration effect.
[0108] Table 3
[0109]
[0110] Test Example 3 Flame retardant properties
[0111] Using a cone calorimeter at 35 kW / m 2Under the conditions, the test was carried out in accordance with the international standard ISO 5660-1 "Reaction to fire test - Heat release, smoke production and mass loss rate, Part 1: Heat release rate (cone calorimeter method)", which includes the test of total ignition time, heat release rate, average carbon monoxide release, average carbon dioxide release, and total smoke release. The results are shown in Table 4. Due to the good penetration behavior of petrification agent and wood particles during the preparation process, silica is not only distributed on the surface and inside the pores of the imitation wood fossil artificial stone board, but also polymerized in situ on the surface of nanofibers inside the wood cell wall, which greatly improves its flame retardant properties.
[0112] contrast Figure 2A and Figure 2B It can be seen that the natural wood is quickly ignited in 12 seconds and produces a lot of smoke, while the imitation wood fossil artificial stone board of the present invention still cannot be ignited within 5 minutes and produces very little smoke.
[0113] Table 4
[0114]
[0115] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a high-strength, water-resistant, flame-retardant wood-like fossil artificial stone board, characterized in that: The artificial stone board imitating wood fossil is prepared by using the petrification agent silica sol to penetrate and gelate in and between wood particles for many times; The preparation method comprises the following steps: 1) Stirring the pretreated wood particles and petrochemical agent, placing the mixture in a mold after uniform mixing, and drying in an oven to obtain an artificial stone slab; 2) The artificial stone slab is completely immersed in the petrochemical agent for 20-40 minutes under a vacuum degree of 1-5 Pa, and then taken out and placed in an oven for drying; 3) Repeat the impregnation-drying operation of step 2) for more than 3 times, so that the petrification agent fully penetrates into and between the wood particles, and gels and grows silica multiple times inside the artificial stone board, and finally obtains the imitation wood fossil artificial stone board; wherein, by volume percentage, the petrochemical agent is composed of 30-60% of ethyl orthosilicate, 10-30% of anhydrous ethanol and 30-50% of water; or The petrochemical agent is composed of 20-80% of ethyl orthosilicate and 20-80% of water; In step 1), 600-800 ml of petrochemical agent is added to every 100 g of wood particles for mixing; The mass proportion of silicon dioxide in the wood-like fossil artificial stone board is 40-70wt%.
2. The preparation method according to claim 1, characterized in that: Calculated by volume percentage, the petrochemical agent consists of 30-50% of ethyl orthosilicate, 10-30% of anhydrous ethanol and 30-50% of water.
3. The preparation method according to claim 1, characterized in that: In step 3), the dipping-drying operation of step 2) is repeated 8-15 times to finally obtain the imitation wood fossil artificial stone board.
4. The preparation method according to claim 1, characterized in that: The drying temperature of the oven is 20-60°C.
5. The preparation method according to claim 1, characterized in that: The mass proportion of silicon dioxide in the wood-like fossil artificial stone board is 53-70wt%.
6. The preparation method according to claim 1, characterized in that: The steps for pre-treating wood particles are: Boil the wood particles in a mixed solution of NaOH and Na2SO3 for 8-12 hours, and then rinse the wood particles with water until they are neutral.
7. A high-strength, water-resistant, flame-retardant artificial stone board imitating fossil wood, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 6.
8. Use of the wood fossil imitation artificial stone board as claimed in claim 7 in the preparation of flame retardant and fireproof building materials.