A titanium-reinforced tailings-bonded corundum refractory material and its preparation method
By preparing titanium-extraction tailings combined with corundum refractory materials, and utilizing titanium-extraction tailings and alumina micro powder to generate CA6 bound phase and solid solution, the problems of resource utilization of titanium-extraction tailings and insufficient performance of corundum refractory materials are solved, achieving high strength and slag erosion resistance, and promoting efficient resource utilization and environmental protection.
Patent Information
- Application Number
- CN202410746860.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing technologies are unable to effectively utilize titanium extraction tailings resources, leading to environmental pollution and resource waste. At the same time, corundum refractory materials lack sufficient sintering densification and slag erosion resistance.
A method for preparing corundum refractory materials using titanium-extracting tailings is adopted. This method uses tabular corundum, titanium-extracting tailings, and alumina powder as raw materials, adds a water-reducing agent, mixes them, casts them into molds, and fires them at high temperature to generate a CA6 bonding phase and a Ca(Al,Mg,Ti)12O19 solid solution, thereby improving the bonding strength and densification effect of the material.
The prepared material has high bulk density, flexural and compressive strength, and slag erosion resistance, achieving efficient resource utilization and environmental protection.
Abstract
Description
Technical Field
[0001] This invention relates to the field of waste treatment and resource utilization technology, and in particular to a titanium tailings-bonded corundum refractory material and its preparation method. Background Technology
[0002] Titanium-iron alloys are widely used due to their ability to refine grain structure and improve steel strength. However, the increasing emissions of titanium-iron slag from titanium-iron alloy smelting lead to solid waste accumulation, severely damaging the environment and wasting resources. To fully utilize the titanium resources in titanium-iron slag, the aluminothermic reduction method is used to extract titanium from it. However, this process still generates a large amount of titanium extraction tailings. Improving the resource utilization efficiency of titanium extraction tailings, reducing solid waste emissions, and conserving resources to achieve sustainable development are of significant practical importance.
[0003] Corundum is currently the most widely used refractory material, possessing excellent high-temperature performance and chemical stability. However, the high purity of corundum bricks leads to difficulties in sintering and insufficient high-temperature bonding strength. Dong Weixia et al. (Dong Weixia, Gu Xingyong, Li Xinhao, et al. Refractory Materials, 2016, 50(6):416-419.) used coal gangue and aluminum hydroxide as the main raw materials, and added 3% metal oxide (V2O5, MnO2 or MgO) additives. After calcination at 1500℃ for 1h, mullite whisker-reinforced corundum refractory materials were generated in situ. Zhu Hui et al. (Zhu Hui, Gong Wei, Li Xiangcheng, et al. Refractory Materials, 2019, 53(4):308-312.) used corundum as the main raw material, aluminate cement as the binder, and added nano alumina powder to promote the formation of CA2 and CA6, thereby improving the thermal shock stability of corundum castables. However, the improvement effect was limited. Moreover, the CA6 generated in the sample after treatment at 1450℃ showed plate-like crystals. The plate-like CA6 overlapped with each other, generating more pores, which was not conducive to sintering and densification. The apparent porosity was close to 20%. Excessive porosity prevents further improvement in material strength and slag erosion resistance. Summary of the Invention
[0004] The purpose of this invention is to address the aforementioned shortcomings of existing technologies by proposing a simple and low-cost method for preparing titanium-tungsten tailings-bonded corundum refractory materials. The titanium-tungsten tailings-bonded corundum refractory material prepared by this invention exhibits high bulk density, high flexural and compressive strength, high high-temperature strength, and excellent resistance to slag erosion.
[0005] The present invention discloses a method for preparing a titanium-extracting tailings-bonded corundum refractory material, comprising using 74-91 wt% tabular corundum, 5-16 wt% titanium-extracting tailings, and 4-10 wt% alumina micro powder as raw materials, adding a water-reducing agent, mixing evenly to obtain a premix; adding water to the premix, stirring evenly, casting into molds, curing at room temperature, demolding, and drying to obtain corundum preforms, and then subjecting them to high-temperature heat preservation to obtain the titanium-extracting tailings-bonded corundum refractory material.
[0006] Furthermore, the high-temperature insulation temperature is 1400–1600℃, and the insulation time is 3–5 hours.
[0007] Furthermore, the drying temperature is 110–120°C.
[0008] Furthermore, the Al2O3 content of the tabular corundum is ≥98wt%; the particle size distribution of the tabular corundum is:
[0009] Particles smaller than 5 mm and greater than or equal to 3 mm account for 30–40 wt% of tabular corundum.
[0010] Particles smaller than 3 mm and greater than or equal to 1 mm account for 40–55 wt% of tabular corundum.
[0011] Particles smaller than 0.088 mm account for 10–22 wt% of tabular corundum.
[0012] Furthermore, the titanium extraction tailings contain Al2O3 ≥ 68 wt%, CaO ≥ 24 wt%, 2 wt% ≥ TiO2 ≥ 1 wt%, and 2 wt% ≥ MgO ≥ 1 wt%.
[0013] Furthermore, the particle size of the titanium extraction tailings is ≤0.044mm.
[0014] Furthermore, the phase composition of the titanium extraction tailings is calcium aluminate CaAl2O4 and calcium aluminate CaAl4O7.
[0015] Furthermore, the alumina micro powder has an Al2O3 content of ≥99wt% and a median diameter of 2μm.
[0016] Furthermore, the water-reducing agent is sodium tripolyphosphate.
[0017] A titanium-containing tailings-bonded corundum refractory material prepared by the above-described preparation method.
[0018] By adopting the above technical solution, the present invention has the following advantages compared with the prior art:
[0019] The raw material selected in this invention, titanium extraction tailings, is abundant and inexpensive, and requires no special processing technology or equipment. Therefore, the process for preparing titanium extraction tailings combined with corundum refractory materials is simple and inexpensive.
[0020] Using tabular corundum as the main raw material, 5-16 wt% of titanium extraction tailings are added as a binder. Water is added, the mixture is stirred, and then cast into shape. During the room temperature curing process, the calcium aluminate (CA) and calcium dialuminate (CA2) in the titanium extraction tailings can react with water to form CAH. 10 Hydration products such as (CaO·Al2O3·10H2O), AH3(Al(OH)3), and C2AH8(2CaO·Al2O3·8H2O) produce high bonding strength; during high-temperature sintering, the above hydration products dehydrate and react with alumina powder to generate calcium hexaaluminate (CaAl) in situ. 12 O 19 The CA6 (Carbonated Iron) phase significantly improves the bonding strength of corundum refractory materials. Furthermore, addressing the issue of CA6's plate-like crystal structure, which creates porosity and hinders sintering and densification, the tailings contain small amounts of TiO2 and MgO. At high temperatures, Ti... 4+ and Mg 2+ It can dissolve in CA6 grains to form Ca(Al,Mg,Ti). 12 O 19 The solid solution promotes the thickening of CA6 lamellar grains, facilitates sintering densification, and thereby reduces the apparent porosity of corundum refractories, improving their mechanical properties and slag erosion resistance.
[0021] The titanium-containing tailings-bonded corundum refractory material prepared by this invention has a bulk density of 3.01–3.11 g·cm³. -3 The room temperature flexural strength is 25–35 MPa; the room temperature compressive strength is 95–135 MPa; the high temperature flexural strength is 17–26 MPa; and the slag erosion index is 9–14%.
[0022] Therefore, the present invention has the characteristics of low cost and simple process; the titanium tailings combined with corundum refractory material prepared has high bulk density, high flexural and compressive strength, good high temperature strength and excellent slag erosion resistance. Detailed Implementation
[0023] The following are specific embodiments of the present invention, which further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0024] To avoid repetition, the materials used in this specific implementation method are described uniformly as follows, and will not be repeated in the examples:
[0025] The Al2O3 content of the tabular corundum is ≥98wt%; the particle size distribution of the tabular corundum is:
[0026] Particles smaller than 5 mm and greater than or equal to 3 mm account for 30–40 wt% of tabular corundum.
[0027] Particles smaller than 3 mm and greater than or equal to 1 mm account for 40–55 wt% of tabular corundum.
[0028] Particles smaller than 0.088 mm account for 10–22 wt% of tabular corundum.
[0029] The titanium extraction tailings contain Al2O3 ≥ 68wt%, CaO ≥ 24wt%, 2wt% ≥ TiO2 ≥ 1wt%, and 2wt% ≥ MgO ≥ 1wt%. The particle size of the titanium extraction tailings is ≤ 0.044mm, and the phase composition of the titanium extraction tailings is calcium aluminate (CA) and calcium dialuminate (CA2).
[0030] The alumina micro powder has an Al2O3 content of ≥99wt% and a median diameter of 2μm.
[0031] The water-reducing agent is sodium tripolyphosphate.
[0032] Example 1
[0033] Using 74 wt% tabular corundum, 16 wt% titanium-extraction tailings, and 10 wt% alumina micro powder as raw materials, a water-reducing agent was added and mixed evenly to obtain a premix. Water was added to the premix, stirred evenly, and cast into molds. After curing at room temperature, demolding, and drying at 110℃, corundum preforms were obtained. After being kept at 1400℃ for 3 hours, titanium-extraction tailings combined with corundum refractory material was obtained.
[0034] The titanium-containing tailings-bonded corundum refractory material prepared in this embodiment was tested and found to have a bulk density of 3.11 g·cm³. -3 The room temperature flexural strength is 35 MPa; the room temperature compressive strength is 135 MPa; the high temperature flexural strength is 26 MPa; and the slag erosion index is 9%.
[0035] Example 2
[0036] Using 80wt% tabular corundum, 13wt% titanium-extraction tailings and 7wt% alumina micro powder as raw materials, a water-reducing agent is added and mixed evenly to obtain a premix. Water is added to the premix, stirred evenly, cast into molds, cured at room temperature, demolded, and dried at 110℃ to obtain corundum preforms. After being kept at 1600℃ for 3 hours, titanium-extraction tailings combined with corundum refractory material is obtained.
[0037] The titanium-containing tailings-bonded corundum refractory material prepared in this embodiment was tested and found to have a bulk density of 3.08 g·cm³. -3 The room temperature flexural strength is 32 MPa; the room temperature compressive strength is 113 MPa; the high temperature flexural strength is 24 MPa; and the slag erosion index is 10%.
[0038] Example 3
[0039] Using 83 wt% tabular corundum, 11 wt% titanium-extraction tailings and 6 wt% alumina micro powder as raw materials, a water-reducing agent is added and mixed evenly to obtain a premix. Water is added to the premix, stirred evenly, cast into molds, cured at room temperature, demolded, and dried at 110℃ to obtain corundum preforms. After being kept at 1600℃ for 3 hours, titanium-extraction tailings combined with corundum refractory material is obtained.
[0040] The titanium-containing tailings-bonded corundum refractory material prepared in this embodiment was tested and found to have a bulk density of 3.05 g·cm³. -3 The room temperature flexural strength is 29 MPa; the room temperature compressive strength is 108 MPa; the high temperature flexural strength is 20 MPa; and the slag erosion index is 12%.
[0041] Example 4
[0042] Using 91 wt% tabular corundum, 5 wt% titanium-extraction tailings and 4 wt% alumina micro powder as raw materials, a water-reducing agent is added and mixed evenly to obtain a premix. Water is added to the premix, stirred evenly, cast into molds, cured at room temperature, demolded, and dried at 110℃ to obtain corundum preforms. After being kept at 1600℃ for 3 hours, titanium-extraction tailings combined with corundum refractory material is obtained.
[0043] The titanium-containing tailings-bonded corundum refractory material prepared in this embodiment was tested and found to have a bulk density of 3.01 g·cm³. -3 The room temperature flexural strength is 25 MPa; the room temperature compressive strength is 95 MPa; the high temperature flexural strength is 17 MPa; and the slag erosion index is 14%.
[0044] For any points not covered above, existing technologies shall apply.
[0045] Although specific embodiments of the present invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art can make various modifications or additions to the described specific embodiments or use similar methods to replace them, without departing from the direction of the invention or exceeding the scope defined by the appended claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc., made to the above embodiments based on the technical essence of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a titanium tailings-bonded corundum refractory material, characterized in that: Using 74-83 wt% tabular corundum, 11-16 wt% titanium-extracting tailings and 6-10 wt% alumina micro powder as raw materials, a water-reducing agent is added and mixed evenly to obtain a premix; water is added to the premix, stirred evenly, cast into molds, cured at room temperature, demolded and dried to obtain corundum preforms, and then subjected to high-temperature heat preservation to obtain titanium-extracting tailings combined corundum refractory material; The high-temperature insulation temperature is 1400~1600 ℃, and the insulation time is 3~5 hours; The Al2O3 content of the tabular corundum is ≥98 wt%; the particle size distribution of the tabular corundum is: Particles smaller than 5 mm and greater than or equal to 3 mm account for 30-40 wt% of tabular corundum. Particles smaller than 3 mm and greater than or equal to 1 mm account for 40-55 wt% of tabular corundum. Particles smaller than 0.088 mm account for 10–22 wt% of tabular corundum; The titanium extraction tailings contain Al2O3 ≥ 68 wt%, CaO ≥ 24 wt%, 2 wt% ≥ TiO2 ≥ 1 wt%, and 2 wt% ≥ MgO ≥ 1 wt%. The particle size of the titanium extraction tailings is ≤ 0.044 mm; The phase composition of the titanium extraction tailings is calcium aluminate CaAl2O4 and calcium aluminate CaAl4O7. The alumina micro powder has an Al2O3 content of ≥99 wt% and a median diameter of 2 μm.
2. The preparation method according to claim 1, characterized in that: The drying temperature is 110~120℃.
3. The preparation method according to claim 1, characterized in that... The water-reducing agent is sodium tripolyphosphate.
4. A titanium-refined tailings-bonded corundum refractory material prepared by the preparation method according to any one of claims 1-3.