Self-repairing scratch-resistant polypropylene and preparation method thereof

Through the combination of modified polypropylene resin and hydroxylated nano-silica, the self-healing ability of polypropylene materials is achieved by using hydrogen bonds, solving the problem of polypropylene materials being susceptible to scratches, and significantly improving the anti-scratch and self-repairing performance , extends service life.

CN118702994BActive Publication Date: 2024-11-08GUANGDONG YONGXINHUA NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411186705.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Existing polypropylene materials are susceptible to scratches during use, resulting in a decrease in appearance quality and shortened service life. The existing scratch-resistant additives can only improve the optical effect and cannot completely eliminate physical scratches.

Method used

The combination of modified polypropylene resin 1 and modified polypropylene resin 2 is adopted, combined with hydroxylated nanosilicon dioxide, and the self-healing ability of the material is achieved through hydrogen bonding and improving damage resistance.

Benefits of technology

It significantly improves the scratch resistance and self-repair properties of polypropylene materials, extends service life, and enhances the toughness and strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a self-repairing scratch-resistant polypropylene and a preparation method thereof. The self-repairing scratch-resistant polypropylene comprises the following components: polypropylene resin, modified polypropylene resin 1, modified polypropylene resin 2, and hydroxylated silica. The various resins have good compatibility, and the modified polypropylene resin 1 containing amino groups and the modified polypropylene resin 2 containing carboxyl groups can form hydrogen bonds for cross-linking. When the polypropylene material is damaged, it can achieve self-repair through hydrogen bonding. In addition, the hydroxylated nano-silica added in the present invention also contains a large number of hydroxyl groups, which can form hydrogen bonds and intermolecular forces with the polar groups in the modified polypropylene resin 1 and the modified polypropylene resin 2, thereby improving the stability of the network cross-linking structure, and further improving the damage resistance of the polypropylene material and the self-repairing effect after damage. The present invention overcomes the shortcomings of the prior art and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic materials, and in particular to self-repairing scratch-resistant polypropylene and a preparation method thereof. Background Art

[0002] Polypropylene (PP) is a polymer material that is non-toxic, low-odor, low-cost, chemically resistant, and has excellent mechanical properties. Due to its excellent performance, polypropylene has been widely used in home appliances, bathrooms, electronics, automobiles, and other fields. In recent years, with the improvement of environmental protection requirements and the development of process technology, the application of spray-free technology in polypropylene materials has become more and more extensive. Spray-free technology not only reduces the production process steps and reduces production costs, but also effectively reduces environmental pollution, which is in line with the concept of green environmental protection.

[0003] Although polypropylene materials have many advantages, there are still some problems in actual use. First, polypropylene products will inevitably be affected by external factors such as cleaning, collision and scratching during use, resulting in slight scratches. These scratches will not only reduce the appearance quality of the product, but also increase the defective rate of the product, affect production efficiency, and significantly reduce the consumer's experience and the actual life of the product.

[0004] In order to reduce visual scratches, the current solution is mainly to add scratch-resistant additives to polypropylene. These additives form a protective layer on the surface of the material, improving the surface slipperiness, so that the brightness change of the scratch after a slight scratch is not obvious. However, this method only improves the optical effect and cannot actually completely eliminate physical scratches, and may even make the scratches deeper.

[0005] In summary, although the existing technology has improved the scratch resistance of polypropylene materials to a certain extent, it is still impossible to completely avoid the generation of scratches. How to fundamentally improve the scratch resistance of polypropylene materials and reduce the impact of scratches on product appearance and service life is still an urgent problem to be solved. Summary of the invention

[0006] Based on this, it is necessary to provide an epoxy resin diffusion plate to overcome the shortcomings of the prior art.

[0007] One object of the present invention is to provide a self-repairing scratch-resistant polypropylene, characterized in that the self-repairing scratch-resistant polypropylene comprises the following components in parts by mass:

[0008] Polypropylene resin 30-65 parts

[0009] Modified polypropylene resin 1 15-40 parts

[0010] Modified polypropylene resin 2 10-30 parts

[0011] Hydroxylated silicon dioxide 15-25 parts

[0012] 1-10 parts of additives.

[0013] Furthermore, the auxiliary agent is selected from one or more of a repairing agent, a dispersant, a heat stabilizer, an antioxidant and a processing aid.

[0014] Furthermore, the repair agent is polyethyleneimine.

[0015] Furthermore, the heat stabilizer is selected from one or more of phenolic heat stabilizers, amine heat stabilizers, phosphite heat stabilizers, and semi-hindered phenolic heat stabilizers.

[0016] Furthermore, the antioxidant is selected from one or more of hindered phenol antioxidants and phosphite antioxidants.

[0017] Furthermore, the processing aid is one or more of low molecular weight esters, metal soaps, stearic acid complex esters and amides.

[0018] Another object of the present invention is to provide a method for preparing the self-repairing scratch-resistant polypropylene, characterized in that it comprises the following steps:

[0019] S1. Adding polyamide and double-terminated carboxyl polypropylene to a solvent, heating the reaction, and purifying to obtain a modified polypropylene resin 1;

[0020] S2. The acrylic acid, polypropylene and initiator are uniformly mixed, melted, extruded and granulated to obtain a modified polypropylene resin 2;

[0021] S3. Adding nano-silica to hydrogen peroxide, heating the reaction, and purifying to obtain hydroxylated nano-silica;

[0022] S4. Mixing the modified polypropylene resin 1, the modified polypropylene resin 2, the hydroxylated nano-silica and other components, melting, extruding and granulating, to obtain the self-repairing scratch-resistant polypropylene.

[0023] Furthermore, in step S1, the heating temperature is 100-120°C.

[0024] Furthermore, in step S2, the reaction temperature is 190-200°C.

[0025] Furthermore, in step S3, the reaction temperature is 60-80°C.

[0026] Furthermore, in step S4, the extrusion temperature is 190-230°C.

[0027] Furthermore, in step S1, the mass ratio of the polyamide to the double-end carboxyl polypropylene is 2-5:1-3.

[0028] Furthermore, in step S2, the mass ratio of acrylic acid to polypropylene is 1-5:8-12.

[0029] The present invention has the following beneficial effects:

[0030] The self-repairing scratch-resistant polypropylene of the present invention is compounded with modified polypropylene resin 1, modified polypropylene resin 2, hydroxylated silica and other components. First, polypropylene is carboxylated, and then cross-linked with polyamide to obtain a modified polypropylene resin 1 having a polypropylene-polyamide block structure, which not only improves the toughness and strength of the material, but also introduces amino groups; the modified polypropylene resin 2 is melted by polypropylene and acrylic acid to introduce polyacrylic acid segments to obtain a modified polypropylene resin 2 with carboxyl groups. The compatibility between the various resins is good, and the modified polypropylene resin 1 containing amino groups and the modified polypropylene resin 2 containing carboxyl groups can form hydrogen bonds for cross-linking. When the polypropylene material is damaged, self-repair can be achieved through hydrogen bonding; in addition, the hydroxylated nano-silica added in the present invention also contains a large number of hydroxyl groups, which can form hydrogen bonds and intermolecular forces with polar groups in the modified polypropylene resin 1 and the modified polypropylene resin 2, thereby improving the stability of the network cross-linked structure, and further improving the damage resistance of the polypropylene material and the self-repairing effect after damage. The present invention overcomes the shortcomings of the prior art and has good application prospects. DETAILED DESCRIPTION

[0031] In order to more clearly illustrate the technical solution of the present invention, the following examples are listed. Unless otherwise stated, the raw materials, reactions and post-treatment methods shown in the examples are common raw materials on the market and technical methods well known to those skilled in the art.

[0032] Polypropylene resin, with a melt index of 25 g / 10 min, was purchased from the South China Branch of Sinopec Chemical Sales Co., Ltd.

[0033] Polyamide, viscosity 20 Pa.s, SF-650-200, purchased from Changzhou Shanfeng Chemical.

[0034] β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, antioxidant, was purchased from Beijing Jiyi Chemical Co., Ltd.

[0035] Heat stabilizer, phenolic heat stabilizer, Irganox 1010, purchased from CIBA.

[0036] Zinc stearate, processing aid.

[0037] Polyethyleneimine, a repair agent, was purchased from Aladdin Reagent Company, with a degree of polymerization of n=15 and n=50.

[0038] Dicumyl peroxide, initiator.

[0039] The raw material components of Examples 1-3 are shown in Table 1, and the numerical values ​​are expressed as mass parts. The "parts" involved in the specification also refer to mass parts.

[0040] Table 1 Composition of the self-repairing scratch-resistant polypropylene of Examples 1-3 (unit: part)

[0041]

[0042] The preparation method of the self-repairing scratch-resistant polypropylene of Examples 1-3 comprises the following steps:

[0043] S1-1. 5 parts of polypropylene and 25 parts of 70wt% concentrated nitric acid were blended, heated to 130°C, stirred for 16h, washed with deionized water and acetone, and dried in vacuo to obtain double-terminated carboxyl polypropylene;

[0044] S1-2. 12 parts of polyamide and 6 parts of double-end carboxyl polypropylene were added to toluene, heated to 110 ° C and refluxed for 22 hours, cooled, precipitated in methanol, and washed with methanol and acetone, and dried in vacuo to obtain a modified polypropylene resin 1;

[0045] S2 10 parts of acrylic acid, 100 parts of polypropylene and 1 part of dicumyl peroxide were mixed uniformly, melted and extruded into granules at 200 ° C by a twin-screw extruder to obtain a modified polypropylene resin 2;

[0046] S3. 7 parts of nano-silica were added to 100 parts of 30wt% hydrogen peroxide, heated to 65 ° C for 5h, washed and dried to obtain hydroxylated nano-silica;

[0047] S4. According to the above mass fractions, the modified polypropylene resin 1, the modified polypropylene resin 2, the hydroxylated nano-silica and other components are mixed, melted and extruded into granules at 200° C. through a twin-screw extruder to obtain the self-repairing scratch-resistant polypropylene.

[0048] Comparative Example 1

[0049] The difference between this comparative example and Example 1 is that: the difference between this comparative example and Example 1 is that: step S1-1 and step S1-2 are removed, a physical mixture of polyamide and polypropylene resin in a mass ratio of 2:1 is used, and the modified polypropylene resin 1 is replaced with an equal mass, and the other ingredients and preparation method are the same as those in Example 1.

[0050] Comparative Example 2

[0051] The difference between this comparative example and Example 1 is that: the difference between this comparative example and Example 1 is that: step S2 is removed, and the modified polypropylene resin 2 is replaced with polypropylene resin of equal mass, and the other components and preparation method are the same as those in Example 1.

[0052] Comparative Example 3

[0053] The difference between this comparative example and Example 1 is that: the difference between this comparative example and Example 1 is that: step S3 is removed, and the hydroxylated nano-silica is replaced with an equal mass of nano-silica, and the other components and preparation method are the same as those in Example 1.

[0054] Test Case

[0055] The performance tests were performed on the polypropylenes prepared in Example 1 and Comparative Examples 1-3.

[0056] The test method is as follows:

[0057] Tensile properties: According to GB / T 1040-2006 standard test, the tensile rate is 50mm / min;

[0058] Scratch resistance and self-repairing performance: Test the scratch resistance of the surface according to GMW14688-2012 standard, and select the scratch force of 10N for the test; calculate the color difference of the performance test before and after the scratching of the polypropylene material surface, as well as the color difference before and 30 minutes after scratching (at 30°C). The smaller the color difference value, the closer the polypropylene surface after scratching is to the state before scratching, and the better its scratch resistance and self-repairing performance.

[0059] Among them, the scratch resistance is tested by calculating the color difference between the performance test before and immediately after scratching;

[0060] The self-healing performance was tested by calculating the color difference between the surface of the polypropylene material before scratching and 30 minutes after scratching.

[0061] The test results are shown in Table 2.

[0062] Table 2 Performance test results of polypropylene in Example 1 and Comparative Examples 1-3

[0063]

[0064] It can be concluded from Table 2 that the polypropylene provided by the present invention has better mechanical properties, scratch resistance and self-repairing properties than the polypropylenes of Comparative Examples 1-3, and has good application prospects.

[0065] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0066] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A self-repairing scratch-resistant polypropylene, It is characterized in that The self-repairing scratch-resistant polypropylene comprises the following components in parts by mass: Polypropylene resin 30-65 parts Modified polypropylene resin 1 22-40 parts Modified polypropylene resin 2 24-30 parts Hydroxylated nano-silicon dioxide 15-25 parts 1-10 parts of additives; The modified polypropylene resin 1 is polyamide-modified polypropylene; The modified polypropylene resin 2 is acrylic acid modified polypropylene; The additive is selected from one or more of a repairing agent, a dispersant, a heat stabilizer and a processing aid; The repair agent is polyethyleneimine; The method for preparing the self-repairing scratch-resistant polypropylene comprises the following steps: S1. Adding polyamide and double-terminated carboxyl polypropylene to a solvent, heating the reaction, and purifying to obtain a modified polypropylene resin 1; S2. The acrylic acid, polypropylene and initiator are uniformly mixed, melted, extruded and granulated to obtain a modified polypropylene resin 2; S3. Adding nano-silica to hydrogen peroxide, heating the reaction, and purifying to obtain hydroxylated nano-silica; S4. Mixing the modified polypropylene resin 1, the modified polypropylene resin 2, the hydroxylated nano-silica and other components, melting, extruding and granulating, to obtain the self-repairing scratch-resistant polypropylene.

2. The self-repairing scratch-resistant polypropylene according to claim 1, It is characterized in that The heat stabilizer is selected from one or more of phenolic heat stabilizers, amine heat stabilizers, phosphite heat stabilizers, and semi-hindered phenolic heat stabilizers.

3. The self-repairing scratch-resistant polypropylene according to claim 1, It is characterized in that In step S1, the heating temperature is 100-120°C; In step S2, the melting temperature is 190-200°C; In step S3, the heating temperature is 60-80°C; In step S4, the extrusion temperature is 190-230°C.

4. The self-repairing scratch-resistant polypropylene according to claim 1, It is characterized in that In step S1, the mass ratio of the polyamide to the double-end carboxyl polypropylene is 2-5:1-3.

5. The self-repairing scratch-resistant polypropylene according to claim 1, It is characterized in that In step S2, the mass ratio of acrylic acid to polypropylene is 1-5:8-12.