A high-air-tightness polyphenylene sulfide-polyamide composite material and its preparation method and application

By adding a specific proportion of components to the polyphenylene sulfide-polyamide composite material and adopting a nano-injection molding process, the airtightness and bonding strength of the material are improved, and the problem of insufficient airtightness in the prior art is solved. It is suitable for The manufacturing of copper/aluminum radiators in new energy vehicles has achieved improved production efficiency and reduced costs.

CN118703041BActive Publication Date: 2024-11-22GUANGZHOU CNDONG NEW MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411178579.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing high heat-resistant polyphenylene sulfide-polyamide composite materials have high failure efficiency in airtightness tests and cannot meet the actual needs of copper discharge/aluminum discharge and filling process of new energy vehicles.

Method used

Polyphenylene sulfide (PPS) 30%-78%, polyamide PA106/10T5%-20%, polyamide copolymer cPA5%-15%, glass fiber 10%-50%, antioxidants 0%-1% , a combination material of 0%-2% mold release agent and 0-6% reactive toughener. High-air-tight composite materials are prepared through nano injection molding process (NMT), and the materials are enhanced through specific polymerization steps and catalyst use. airtightness and bonding power.

Benefits of technology

It realizes polyphenylene sulfide-polyamide composite materials with high airtightness and high binding force in the nanoinjection molding process of copper and aluminum, solves the problems of long production cycle, unfriendly environment and high cost, and is suitable for large-scale production. and reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118703041B_ABST
    Figure CN118703041B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of composite materials, and discloses a high-air-tightness polyphenylene sulfide-polyamide composite material, a preparation method thereof, and an application thereof. The composite material comprises the following components in weight percentage: polyphenylene sulfide 30-78%; polyamide PA106 / 10T 5-20%; polyamide copolymer cPA 5-15%, glass fiber 10-50%; antioxidant 0-1%; release agent 0-2%; reactive toughening agent 0-6%. The polyphenylene sulfide-polyamide composite material of the present invention has good air tightness with metal in the nano injection molding process (NMT), and the material has extremely high bonding strength with the nano injection molding of copper and aluminum, which solves the shortcomings of long production cycle and environmental unfriendly glue filling process in the production of copper / aluminum bars in the current three-electric system of new energy vehicles. At the same time, the preparation method of the present invention is simple and easy to implement, suitable for large-scale production, and can reduce costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and particularly relates to a high-air-tightness polyphenylene sulfide-polyamide composite material and a preparation method and application thereof. Background Art

[0002] With the development of electric vehicles, the three-electric system consisting of motors, electronic controls and batteries has become the core component of electric vehicles. As an important part of circuit connection, copper busbars / aluminum busbars occupy a very important position in the three-electric system. Copper busbars / aluminum busbars are mainly composed of copper plates / aluminum plates and plastic shell injection molding, and need to have properties such as resistance to cold and hot shocks, high temperature resistance, and insulation. At present, the plastic shell of copper busbars / aluminum busbars is mainly composed of polyphenylene sulfide PPS or high-temperature polyamide PPA. At the same time, in order to ensure the sealing of the joint between the metal plate and the plastic, the copper busbars / aluminum busbars need to be glued. The glue pouring process has the disadvantages of being environmentally unfriendly, having a long production cycle and high cost. The use of nano injection molding NMT process to achieve the sealing of the joint between metal and plastic parts can improve the shortcomings of the glue pouring process, improve production efficiency and reduce costs. Patent CN202211118208.4 reports a high-heat-resistant polyphenylene sulfide-polyamide composite material that can be applied to both copper and aluminum NMT processes, solving the problem of low bonding strength of the NMT process. However, in actual production, it was found that both the material in the patent and other PPS materials on the market had a high failure rate in the air tightness test and could not meet the actual production needs of replacing glue filling. Summary of the invention

[0003] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a polyphenylene sulfide-polyamide composite material with better air tightness that can be used for nano-injection molding of copper and aluminum, while ensuring that the material has a higher bonding strength with the nano-injection molding of copper and aluminum, thereby solving the current problems.

[0004] Another object of the present invention is to provide a method for preparing the above-mentioned high airtightness polyphenylene sulfide-polyamide composite material.

[0005] Another object of the present invention is to provide an application of the above-mentioned high-airtightness polyphenylene sulfide-polyamide composite material in the manufacture of copper bars / aluminum bars for new energy vehicles.

[0006] The purpose of the present invention is achieved through the following solutions:

[0007] A high-air-tightness polyphenylene sulfide-polyamide composite material, comprising the following components in percentage by weight:

[0008] Polyphenylene sulfide (PPS) 30%-78%;

[0009] Polyamide PA106 / 10T 5%-20%;

[0010] Polyamide copolymer cPA 5%-15%;

[0011] Glass fiber 10%-50%;

[0012] Antioxidant 0%-1%;

[0013] Release agent 0%-2%;

[0014] Reactive toughening agent 0-6%;

[0015] The polyamide PA106 / 10T is obtained by copolymerizing adipic acid, terephthalic acid and decanediamine, wherein the molar ratio of adipic acid to terephthalic acid is 6:4 to 3:7, preferably 5:5.

[0016] The polyamide copolymer cPA is copolymerized by monomer A, monomer B and monomer C, wherein the weight of monomer A, monomer B and monomer C accounts for 60%-80%, 10%-20% and 10-20% of the total weight of the three monomers (monomer A, monomer B and monomer C) respectively. The monomer A is a blend of decanediamine and aliphatic dibasic acid, and the molar ratio of decanediamine and aliphatic dibasic acid adipic acid is (0.98-1.02):1; the monomer B is a mixture of polytetrahydrofuran diamine with a molecular weight of 900-1500 and aliphatic dibasic acid, and the molar ratio of polytetrahydrofuran diamine and aliphatic dibasic acid in the monomer B is (0.98-1.02):1; the monomer C is a mixture of alicyclic monomer and aliphatic dibasic acid. The compound, the alicyclic monomer is one of MACM (3,3'-dimethyl-4,4-diaminodicyclohexylmethane) and PACM (4,4'-diaminodicyclohexylmethane), the molar ratio of the alicyclic monomer to the aliphatic dibasic acid in the monomer C is (0.98-1.02):1; the aliphatic dibasic acid in the monomer A, the monomer B and the monomer C are all relatively independently at least one of succinic acid, adipic acid and azelaic acid, and are all preferably adipic acid.

[0017] Preferably, in the polyamide copolymer cPA, the mass ratios of monomer A, monomer B and monomer C to the total mass of the three monomers (monomer A, monomer B and monomer C) are 75%, 10% and 15% respectively.

[0018] The polyamide copolymer cPA is prepared by the following method:

[0019] Step 1: Add monomers A, B, C and catalyst into a polymerization reactor;

[0020] Step 2: Nitrogen purging, the pressure is maintained at 0.3-1.0MPa;

[0021] Step 3: Heat the solution to 100-140°C and stir for 1-3h;

[0022] Step 4: Continue to heat up to 220-260℃ and maintain pressure for 1-3h;

[0023] Step 5: The pressure is reduced to 0 MPa, and the material is discharged after vacuuming for 5-240 minutes to obtain a transparent nylon elastomer, i.e., a polyamide copolymer cPA.

[0024] The catalyst in step 1 is one or a mixture of hypophosphorous acid, phosphoric acid, and hypophosphite. The amount of the catalyst is such that the weight of the catalyst accounts for 0.05-0.2% of the total weight of the three monomers.

[0025] The antioxidant is at least one of hindered phenol antioxidants, hindered amine antioxidants, and cuprous salt antioxidants, and is preferably antioxidant 1098.

[0026] The weight percentage of the antioxidant is preferably 0.05%-1%.

[0027] The release agent is at least one of polyvinyl alcohol, long-chain fatty acid ester and long-chain fatty acid amide, preferably Nylostab S-EED from Clariant.

[0028] The weight percentage of the release agent is preferably 0.1%-2%.

[0029] The reactive toughening agent is one or both of a toughening agent containing maleic anhydride and a toughening agent containing glycidyl ether; wherein the toughening agent containing maleic anhydride is one or both of maleic anhydride copolymerized with ethylene methyl acrylate and maleic anhydride grafted with ethylene octene copolymer, and the toughening agent containing glycidyl ether is one or both of ethylene methyl acrylate glycidyl ether copolymer and ethylene glycidyl ether copolymer.

[0030] Preferably, the reactive toughening agent is a mixture of a toughening agent containing maleic anhydride and a toughening agent containing glycidyl ether, wherein the weight ratio of the toughening agent containing maleic anhydride to the toughening agent containing glycidyl ether is 3:1~1:1, preferably 2~1; wherein the toughening agent containing maleic anhydride is preferably maleic anhydride copolymerized with ethylene methyl acrylate, and the toughening agent containing glycidyl ether is preferably ethylene methyl acrylate glycidyl ether copolymer.

[0031] Preferably, the amount of the reactive toughening agent is 3-6%.

[0032] Preferably, the polyphenylene sulfide-polyamide composite material may also contain aluminum diethylphosphinate and aluminum phosphite, the total weight percentage of aluminum diethylphosphinate and aluminum phosphite is 0.1% to 0.8%, preferably 0.1% to 0.5%; wherein the mass ratio of aluminum diethylphosphinate to aluminum phosphite is 4:1.

[0033] A method for preparing the above-mentioned high-air-tightness polyphenylene sulfide-polyamide composite material comprises the following steps: mixing the components and extruding and granulating them through an extruder, and the granulation temperature is 280-320°C.

[0034] The above-mentioned high-airtightness polyphenylene sulfide-polyamide composite material is used in the manufacture of copper / aluminum busbars of the three-electric system of new energy vehicles through nano injection molding process (NMT).

[0035] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0036] The polyphenylene sulfide-polyamide composite material of the present invention has good airtightness in the nano-injection molding (NMT) process of copper and aluminum, and the material has high bonding strength with the nano-injection molding of copper and aluminum, which solves the shortcomings of the current copper / aluminum busbar glue filling process of the three-electric system of new energy vehicles, such as long production cycle and environmental unfriendliness. At the same time, the preparation method of the present invention is simple and easy to implement, suitable for large-scale production, and can reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of the structure of the plastic test piece, where 1 represents the metal part (copper or aluminum) and 2 represents the plastic part.

[0038] Figure 2 It is a schematic diagram of the structure of the copper busbar / aluminum exhaust tightness test unit, where 1 is a copper sheet or an aluminum sheet, 2 is a plastic part, 3 is a test fixture used to combine with the plastic part to form a test cavity, and 4 is an air filling port. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0040] The technical solution of the present application is described in detail using an embodiment. The preparation method of polyamide PA106 / 10T in the embodiment is as follows: adipic acid, terephthalic acid and decanediamine are input into a polymerization kettle, the molar ratio of acid to amine is 1:1, and the polymerization kettle is heated and stirred for dehydration reaction (the pressure of the polymerization kettle is 25 bar and the temperature is 320°C). After complete reaction, the polyamide melt is discharged, and the melt is molded by a die casting strip, and is obtained by cooling and pelletizing. For details, see the patent application "CN202110716096.1-A polyamide and its preparation method". In the embodiment, PA106 / 10T (5:5) means that the molar ratio of adipic acid to terephthalic acid is 5:5.

[0041] The preparation method of the polyamide copolymer cPA in the embodiment is: Add monomers A, B, C and the catalyst hypophosphorous acid to the polymerization kettle; nitrogen purge, and keep the pressure at 0.5MPa; heat the solution to 120°C and stir at a constant temperature for 2h; continue to heat to 240°C and keep the pressure for 2h; the pressure is reduced to 0MPa, and the material is discharged after vacuuming for 90min to obtain the polyamide copolymer cPA. The molar ratio of decanediamine to aliphatic dibasic acid in monomer A is 1.02:1; the molecular weight of polytetrahydrofuran diamine in monomer B is 1000, and the molar ratio of polytetrahydrofuran diamine to aliphatic dibasic acid is 1:1; the molar ratio of MACM to aliphatic dibasic acid in monomer C is 1:1. The amount of the catalyst hypophosphorous acid added is 0.1% of the total weight of the three monomers. See patent application "CN202311374296.9 A transparent nylon elastomer and its preparation method" for details.

[0042] The remaining raw materials in the embodiment can be obtained from the market, specifically as follows: polyphenylene sulfide is CXP-500C from Zhuhai Changxian, glass fiber is ECS3031H from Chongqing International, maleic anhydride copolymerized with polyethylene methyl acrylate is A560 from DuPont, ethylene methyl acrylate glycidyl ether copolymer is AX8900 from Arkema, antioxidant 1098 is Tianjin Lianlong 1098, release agent is NylostabS-EED from Clariant, and aluminum diethylphosphinate / aluminum phosphite (4:1) is OP1400 from Clariant.

[0043] The aluminum nano-injection molded aluminum specimen used in the present invention is prepared by the following process: high-purity aluminum material, size specifications are length 45mm, width 18mm, thickness 1.6mm; T treatment process: sequentially immerse in NaOH solution alkaline washing (1mol / L, 30 seconds), hydrochloric acid corrosion (1mol / L, 5 minutes), and ammonia solution (T treatment solution, 0.5mol / L, 2 minutes), and then the immersed specimen is cleaned with water and dried to obtain an aluminum specimen with nanopores on the surface.

[0044] The copper nano-injection molded copper sample used in the present invention is prepared by the following process: brass material, size specifications are length 45mm, width 18mm, thickness 1.6mm; T treatment process: sequentially immerse in NaOH solution alkaline washing (1mol / L, 30 seconds), nitric acid corrosion (1.5mol / L, 5 minutes), and ammonia solution (T treatment solution, 0.5mol / L, 2 minutes), and then the immersed sample is cleaned with water and dried to obtain a copper sample with nanopores on the surface.

[0045] Preparation of the plastic metal test monolith used in the present invention:

[0046] The present invention refers to the method of Japanese Taisei Nano Injection Molding related patent (US8057890 (B2)) to prepare the plastic metal test integral part. Figure 1 This is a schematic diagram of the structure of the plastic-metal test piece. The size of the metal sheet is 18mm×45mm×1.6mm, the size of the plastic part is 10mm×45mm×3mm, and the bonding area between the plastic and the metal is 0.5cm 2 In all experiments, the injection molding maintained the same injection molding conditions, barrel temperature 290-320°C, mold temperature 140°C, and the polyphenylene sulfide-polyamide composite material was injected onto the metal sheet to obtain a plastic-metal test integral part.

[0047] Plastic-metal bonding performance test:

[0048] The plastic-metal bonding strength test standard used in the present invention refers to the standard in Japan's Daisei Chemical patent (US8057890 (B2)), and the plastic-metal bonding area is 0.5cm 2 , perform biaxial tensile test on the plastic metal test piece.

[0049] The schematic diagram of the structure of the copper busbar / aluminum exhaust tightness test unit in the present invention is as follows: Figure 2 As shown, 1 is a copper or aluminum sheet, 15mm wide, 140mm long (the fold is in the middle), and 2mm thick; 2 is a plastic part, 150mm long, 90mm wide, and 60mm high; 3 is a test fixture, used to combine with the plastic part to form a test cavity, and 4 is an inflation port. 1 is combined with 2 by injection molding, and 2 and 3 are combined under pressure by a sealing strip. The airtightness test method used is: Figure 2 The test piece shown is inflated through the inflation port, the pressure is increased to 0.5 bar, the pressure increase process lasts for 30 seconds, the pressure is maintained for 30 seconds, the pressure is stopped, and the gas leakage rate is tested. The test equipment used is the Wanken Leakage Tester T-89. During the test, the plastic part and the test fixture are sealed by a rubber ring.

[0050] Comparative Example 1 and Examples 1-7

[0051] The polyphenylene sulfide-polyamide composite materials in Comparative Example 1 and Examples 1-7 are prepared by the following steps: weighing the corresponding amounts of components by weight, then mixing the components, and granulating the polyphenylene sulfide-polyamide composite materials using a twin-screw extruder, and the granulation temperature is 260-320°C. Among them, the composition of the three monomers of the polyamide copolymer cPA used in Examples 1-7 and the content of the three monomers (i.e., the percentage (%) of the total weight of the three monomers) are shown in Table 1. The weight percentages of the components in Comparative Example 1 and Examples 1-7 and the various properties of the prepared polyphenylene sulfide-polyamide composite materials are shown in Table 2 below.

[0052] Table 1. Composition information of polyamide copolymer cPA used in Examples 1-7

[0053]

[0054] Table 2. Comparison of weight fractions of each component in Comparative Example 1 and Examples 1-7 and various properties of the prepared polyphenylene sulfide-polyamide composite materials

[0055]

[0056] It can be seen from the data in Table 2 that when the weight ratio of A, B, and C in cPA is 70%, 15%, and 15%, and the aliphatic dibasic acid in monomer A, monomer B, and monomer C is adipic acid, the polyphenylene sulfide-polyamide composite material has the lowest leakage rate and the highest bonding strength. Since the leakage rate required by production is less than 0.5 ml / min, only Example 2 can meet the requirements of mass production.

[0057] Examples 8-12

[0058] The polyphenylene sulfide-polyamide composite materials in Examples 8-12 are prepared by the following steps: weighing the corresponding amount of components by weight, then mixing the components, and granulating the polyphenylene sulfide-polyamide composite materials using a twin-screw extruder, and the granulation temperature is 280-320° C. Among them, the weight percentages of the components in Example 2 and Examples 8-12 and the various properties of the prepared polyphenylene sulfide-polyamide composite materials are shown in Table 3 below.

[0059] Table 3. Comparison of weight fractions of each component in Example 2 and Examples 8-12 and various properties of the prepared polyphenylene sulfide-polyamide composite materials

[0060]

[0061] As shown in Table 3, when the content of cPA is 15 parts or less and the content of PA106 / 10T is 20 parts or less, higher NMT bonding strength and air tightness can be obtained at the same time.

[0062] By comparing Example 2 (the content of cPA is 10 parts, the content of PA106 / 10T is 10 parts) with Comparative Example 1 (the content of cPA is 0 parts, the content of PA106 / 10T is 20 parts) and Example 9 (the content of cPA is 20 parts, the content of PA106 / 10T is 0 parts), it can be seen that the bonding force between the composite material obtained in Example 2 and aluminum and copper is higher than that of Comparative Example 1 and Example 9, and the leakage rate is also slower than that of Comparative Example 1 and Example 9, indicating that there is a synergistic effect between cPA2 and PA106 / 10T.

[0063] Examples 13-19

[0064] The polyphenylene sulfide-polyamide composite materials in Examples 13-19 are prepared by the following steps: weighing the corresponding amount of components by weight, then mixing the components, and granulating the polyphenylene sulfide-polyamide composite materials using a twin-screw extruder, and the granulation temperature is 280-320° C. The weight percentages of the components in Examples 13-19 and the various properties of the prepared polyphenylene sulfide-polyamide composite materials are shown in Table 4 below.

[0065] Table 4. Comparison of weight fractions of each component in Examples 13-19 and various properties of the prepared polyphenylene sulfide-polyamide composite materials

[0066]

[0067] From the data in Table 4, it can be seen that adding a suitable amount of reactive toughening agent and / or OP1400 to the system can further improve the NMT bonding strength and air tightness of the polyphenylene sulfide-polyamide composite.

[0068] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A high airtightness polyphenylene sulfide-polyamide composite material, characterized in that The composition comprises the following components in weight percentage: Polyphenylene sulfide 30%-78%; Polyamide PA106 / 10T 5%-20%; Polyamide copolymer cPA 5%-15%; Glass fiber 10%-50%; Antioxidant 0%-1%; Release agent 0%-2%; Reactive toughening agent 0-6%; The polyamide PA106 / 10T is obtained by copolymerizing adipic acid, terephthalic acid and decanediamine, wherein the molar ratio of adipic acid to terephthalic acid is 6:4 to 3:7; The polyamide copolymer cPA is copolymerized by monomer A, monomer B and monomer C, wherein the monomer A is a blend of decanediamine and an aliphatic dibasic acid; the monomer B is a mixture of polytetrahydrofuran diamine and an aliphatic dibasic acid; the monomer C is a mixture of an alicyclic monomer and an aliphatic dibasic acid, and the alicyclic monomer is one of MACM and PACM; The weight ratios of monomer A, monomer B and monomer C to the total weight of the three monomers are 60%-80%, 10%-20% and 10-20% respectively.

2. The high airtightness polyphenylene sulfide-polyamide composite material according to claim 1, characterized in that: In monomer B, the number average molecular weight of polytetrahydrofuran diamine is 900-1500; The aliphatic dibasic acid in monomer A, monomer B and monomer C is independently at least one of succinic acid, adipic acid and azelaic acid; The monomer A is a blend of decanediamine and an aliphatic dibasic acid, and the molar ratio of decanediamine to the aliphatic dibasic acid is (0.98-1.02):1; the molar ratio of polytetrahydrofuran diamine to the aliphatic dibasic acid in the monomer B is (0.98-1.02):1; the molar ratio of alicyclic monomer to the aliphatic dibasic acid in the monomer C is (0.98-1.02):

1.

3. The high airtightness polyphenylene sulfide-polyamide composite material according to claim 1, characterized in that: In the polyamide copolymer cPA, the weight ratios of monomer A, monomer B and monomer C to the total weight of the three monomers are 75%, 10% and 15% respectively; the aliphatic dibasic acids in monomer A, monomer B and monomer C are all adipic acid.

4. The high airtightness polyphenylene sulfide-polyamide composite material according to claim 1, characterized in that: The antioxidant is at least one of a hindered phenol antioxidant, a hindered amine antioxidant, and a cuprous salt antioxidant; The release agent is at least one of polyvinyl alcohol, long-chain fatty acid ester and long-chain fatty acid amide; The weight percentage of the antioxidant is 0.05%-1%; The weight percentage of the release agent is 0.1%-2%.

5. The high airtightness polyphenylene sulfide-polyamide composite material according to claim 1, characterized in that: The reactive toughening agent is one or both of a toughening agent containing maleic anhydride and a toughening agent containing glycidyl ether; wherein the toughening agent containing maleic anhydride is one or both of maleic anhydride copolymerized with polyethylene methyl acrylate and maleic anhydride grafted with ethylene octene copolymer; and the toughening agent containing glycidyl ether is AX8900 of Arkema Company.

6. The high airtightness polyphenylene sulfide-polyamide composite material according to claim 1, characterized in that: The reactive toughening agent is a mixture of a toughening agent containing maleic anhydride and a toughening agent containing glycidyl ether, wherein the weight ratio of the toughening agent containing maleic anhydride to the toughening agent containing glycidyl ether is 3:1-1:

1.

7. The high airtightness polyphenylene sulfide-polyamide composite material according to claim 1, characterized in that: The polyphenylene sulfide-polyamide composite material also contains aluminum diethylphosphinate and aluminum phosphite, and the total weight percentage of aluminum diethylphosphinate and aluminum phosphite is 0.1% to 0.8%; wherein the mass ratio of aluminum diethylphosphinate to aluminum phosphite is 4:

1.

8. A method for preparing a high-airtightness polyphenylene sulfide-polyamide composite material according to any one of claims 1 to 7, characterized in that The method comprises the following steps: mixing the components and extruding and granulating the components through an extruder, wherein the granulating temperature is 280-320°C.

9. Use of the high-airtightness polyphenylene sulfide-polyamide composite material according to any one of claims 1 to 7 in manufacturing copper or aluminum bars of the three-electric system of new energy vehicles.