Domestication method of ethylene epoxidized silver catalyst

By using specific domestication steps in the ethylene silver epoxide catalyst, including temperature rise desorption and heat treatment, the problem of high impurities on the catalyst surface and unstable active surface area is solved, the efficiency and stability of the catalyst are improved, and the efficiency of ethylene oxide is improved. yield and selectivity.

CN118719059APending Publication Date: 2024-10-01REZEL CATALYSTS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410715522.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing silver catalysts have many surface impurities and unstable active surface area during the ethylene epoxidation process, resulting in low yield and selectivity, and require domestication treatment to improve their efficiency and stability in industrial production.

Method used

Place the ethylene epoxide silver catalyst to be domesticated in the reaction system under an inert gas atmosphere, desorb the amine compounds and oxygen by raising the temperature, inject dichloroethane for adsorption, and then perform heat treatment at a specific temperature and pressure to combine with carbon dioxide and oxygen to control working conditions to complete acclimation.

Benefits of technology

Through this method, the activity and stability of the catalyst were successfully improved, the yield and selectivity of ethylene oxide were improved, and the gap in the existing silver catalyst domestication technology was filled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719059A_ABST
    Figure CN118719059A_ABST
Patent Text Reader

Abstract

The invention relates to a domestication method of an ethylene epoxidized silver catalyst, and relates to the technical field of domestication of silver catalysts, the domestication method comprises the following steps: in an inert gas atmosphere, placing the ethylene epoxidized silver catalyst to be domesticated in a reaction system, and then heating the reaction system to 207-212 DEG C for desorption of amine compounds on the surface of the catalyst; heating the reaction system to 215-220 DEG C, introducing ethylene to perform oxygen desorption on the surface of the catalyst, and injecting 2-5ppm dichloroethane to perform adsorption; after saturated adsorption is achieved, the temperature and pressure of a reaction system are kept unchanged, the concentration of dichloroethane is reduced to 0.5-0.9 ppm, carbon dioxide with the volume percentage being 0.2-0.4% is added firstly, then oxygen is slowly added to 3%, and the like. The invention provides a domestication method of an ethylene epoxidized silver catalyst. The domestication method fills the blank of an existing silver catalyst domestication technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silver catalyst domestication, in particular to a domestication method for an ethylene epoxidation silver catalyst. Background Art

[0002] Ethylene oxide is an important organic compound, mainly used to produce ethylene glycol, which is the main raw material for producing polyester products (such as polyester fiber, polyester film, polyester plastic, etc.), accounting for about 90% of ethylene glycol consumption. Ethylene oxide is also used to produce rubber, plastics, plasticizers and lubricants, and is widely used in many fields such as laundry, electronics, medicine, pesticides, textiles, papermaking, automobiles, oil extraction and refining, etc.

[0003] In the reaction of ethylene epoxidation to produce ethylene oxide in industry, a mixed gas containing ethylene and oxygen produces ethylene oxide under certain reaction conditions under the action of a silver-silver catalyst, and at the same time produces a small amount of by-products such as carbon dioxide and water. At present, the silver-silver catalyst is still the only effective silver catalyst widely used in actual production in the field of ethylene epoxidation in industry. The silver catalyst usually uses alumina as a carrier and silver as an active component, and contains certain other elements of additives and co-additives to improve its catalytic performance. The silver-silver catalyst is a supported gas-solid reaction silver catalyst used for direct oxidation of ethylene to produce ethylene oxide. However, since silver is the main catalyst and other co-catalysts, it is loaded on the surface of the carrier to form an active component. The surface of the newly produced silver-silver catalyst is not clean, and many impurities are adsorbed, so the ethylene epoxidation reaction cannot occur directly. The active surface area is also unstable and prone to temperature runaway. It needs to be acclimated under working conditions. Through a reasonable acclimation process, the efficiency and stability of the silver catalyst in actual industrial production can be ensured, and the yield and selectivity of the product can be improved. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a method for taming an ethylene epoxide silver catalyst.

[0005] The present invention provides a method for taming an ethylene epoxide silver catalyst, the method comprising the following steps:

[0006] Under an inert gas atmosphere, placing the ethylene epoxide silver catalyst to be acclimated in a reaction system, and then heating the reaction system to 207-212° C. to desorb the amine compounds on the catalyst surface;

[0007] The reaction system was heated to 215-220°C and ethylene was introduced to desorb oxygen from the catalyst surface, and then 2-5 ppm of ethylene dichloride was injected for adsorption;

[0008] After reaching saturated adsorption, the temperature and pressure of the reaction system remain unchanged, the concentration of dichloroethane is reduced to 0.5-0.9 ppm, 0.2-0.4% of carbon dioxide by volume is first added, and then oxygen is slowly added to 3%. Under this working condition, the reaction temperature is raised to 235-240°C for acclimation for 40-52 hours to complete the acclimation.

[0009] Furthermore, the desorption temperature of the amine compounds on the catalyst surface is 210°C.

[0010] Furthermore, the temperature of oxygen desorption on the catalyst surface is 218°C.

[0011] Furthermore, the acclimation chlorine injection concentration is 3.9 ppm.

[0012] Furthermore, the acclimation temperature is 238°C.

[0013] Furthermore, the acclimatization time is 48 hours.

[0014] Furthermore, after the acclimation is completed, the temperature is lowered to 218°C, the air velocity remains unchanged, the ethylene concentration is increased to 30%, and the oxygen concentration is slowly increased, and the ethylene oxide concentration in the tail gas will rise synchronously.

[0015] Further, in terms of weight percentage, the composition of the ethylene epoxide silver catalyst comprises:

[0016] Silver: 21-33%;

[0017] One or more alkali metals: 0-0.3%;

[0018] One or more alkaline earth metals: 0-0.3%;

[0019] One or more metals of Group VIIB: 0-0.31%;

[0020] Aluminum oxide: 67-79%.

[0021] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:

[0022] The embodiment of the present invention provides a method for taming an ethylene epoxidation silver catalyst. The method determines the dichloroethane concentration during taming, the chlorine injection time and temperature, the heat treatment time and temperature, and the dichloroethane concentration during heat treatment through experiments, thus filling the gap in the existing silver catalyst taming technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0025] Figure 1 A schematic flow chart of a method for acclimating an ethylene epoxide silver catalyst provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0028] In the first aspect, the present invention provides a method for taming an ethylene epoxide silver catalyst, such as Figure 1 As shown, the domestication method comprises the following steps:

[0029] Under an inert gas atmosphere, placing the ethylene epoxide silver catalyst to be acclimated in a reaction system, and then heating the reaction system to 207-212° C. to desorb the amine compounds on the catalyst surface;

[0030] The reaction system was heated to 215-220°C and ethylene was introduced to desorb oxygen from the catalyst surface, and then 2-5 ppm of ethylene dichloride was injected for adsorption;

[0031] After reaching saturated adsorption, the temperature and pressure of the reaction system remain unchanged, the concentration of dichloroethane is reduced to 0.5-0.9 ppm, 0.2-0.4% of carbon dioxide by volume is first added, and then oxygen is slowly added to 3%. Under this working condition, the reaction temperature is raised to 235-240°C for acclimation for 40-52 hours to complete the acclimation.

[0032] The embodiment of the present invention provides a method for taming an ethylene epoxide silver catalyst. The embodiment of the present invention provides a method for taming an ethylene epoxide silver catalyst. The method determines the dichloroethane concentration during taming, the chlorine injection time and temperature, the heat treatment time and temperature, and the dichloroethane concentration during heat treatment through experiments, thus filling the gap in the existing silver catalyst taming technology.

[0033] In some specific embodiments, the temperature for desorption of amine compounds on the catalyst surface is 210°C.

[0034] In some specific embodiments, the temperature of oxygen desorption on the catalyst surface is 218°C.

[0035] In some specific embodiments, the acclimation chlorine injection concentration is 3.9 ppm.

[0036] In some specific embodiments, the acclimation temperature is 238°C.

[0037] In some specific embodiments, the acclimation time is 48 hours.

[0038] In some specific embodiments, after the acclimation is completed, the temperature is lowered to 218° C., the space velocity remains unchanged, the ethylene concentration is increased to 30%, and the oxygen concentration is slowly increased, and the ethylene oxide concentration in the tail gas will rise synchronously.

[0039] In some specific embodiments, the ethylene epoxide silver catalyst can be selected from RS8910A silver catalyst of Runhe Catalyst Co., Ltd. In terms of weight percentage, the composition of the ethylene epoxide silver catalyst includes:

[0040] Silver: 27wt%;

[0041] Cesium: 0.1wt%;

[0042] Strontium: 0.1wt%;

[0043] Rhenium: 0.1wt%;

[0044] Aluminum oxide: 72.7%.

[0045] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0046] Example 1

[0047] This example provides a method for taming an ethylene epoxide silver catalyst. Taking Runhe RS8910A silver catalyst as an example, the taming method of the ethylene epoxide silver catalyst comprises the following steps:

[0048] 1 ml of silver catalyst was loaded into the reactor and the temperature was raised to 210°C under a nitrogen atmosphere. It was considered that the amines on the surface of the silver catalyst had been desorbed completely at this time; the temperature was raised to 218°C and 15% ethylene was slowly introduced to take away the surface adsorbed oxygen; the temperature was kept constant and 2.5 ppm of dichloroethane was injected for 17 hours, which was considered to have just reached saturated adsorption.

[0049] The system temperature and pressure remain unchanged, and the concentration of ethylene dichloride is reduced to 0.7ppm. First, 0.3% carbon dioxide is added, and then oxygen is slowly added to 3%. Under this low-load condition, no ethylene oxide component is detected in the exhaust gas, indicating that at this time all the ethylene dichloride is adsorbed on the active surface, no oxygen is adsorbed, and no epoxidation reaction of ethylene occurs.

[0050] Under this working condition, the reaction temperature rises to 238°C and is maintained for 48 hours to complete the acclimatization.

[0051] After the acclimation is completed, the temperature is lowered to 218°C, the air velocity remains unchanged, the ethylene concentration is increased to 30%, and the oxygen concentration is slowly increased. The ethylene oxide concentration in the tail gas will rise synchronously.

[0052] Example 2

[0053] On the basis of Example 1, the dichloroethane concentration during acclimation, the chlorine injection time and temperature, the heat treatment time and temperature, and the dichloroethane concentration during heat treatment were screened in this example. The results are shown in Table 1.

[0054] Table 1

[0055]

[0056]

[0057] In summary, the embodiment of the present invention provides a method for taming an ethylene epoxide silver catalyst. The method determines the dichloroethane concentration during taming, the chlorine injection time and temperature, the heat treatment time and temperature, and the dichloroethane concentration during heat treatment through experiments, thus filling the gap in the existing silver catalyst taming technology.

[0058] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0059] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for acclimating an ethylene epoxide silver catalyst, characterized in that: The domestication method comprises the following steps: Under an inert gas atmosphere, placing the ethylene epoxide silver catalyst to be acclimated in a reaction system, and then heating the reaction system to 207-212° C. to desorb the amine compounds on the catalyst surface; The reaction system was heated to 215-220°C and ethylene was introduced to desorb oxygen from the catalyst surface, and then 2-5 ppm of ethylene dichloride was injected for adsorption; After reaching saturated adsorption, the temperature and pressure of the reaction system remain unchanged, the concentration of dichloroethane is reduced to 0.5-0.9 ppm, 0.2-0.4% of carbon dioxide by volume is first added, and then oxygen is slowly added to 3%. Under this working condition, the reaction temperature is raised to 235-240°C for acclimation for 40-52 hours to complete the acclimation.

2. The acclimation method according to claim 1, characterized in that: The desorption temperature of amine compounds on the catalyst surface is 210℃.

3. The acclimation method according to claim 1, characterized in that: The temperature of oxygen desorption on the catalyst surface is 218℃.

4. The acclimation method according to claim 1, characterized in that: The chlorine injection concentration for acclimatization is 3.9ppm.

5. The acclimation method according to claim 4, characterized in that: The acclimatization temperature is 238℃.

6. The acclimation method according to claim 1, characterized in that: The acclimatization time is 48 hours.

7. The acclimation method according to claim 1, characterized in that: After the acclimation is completed, the temperature is lowered to 218°C, the air velocity remains unchanged, the ethylene concentration is increased to 30%, and the oxygen concentration is slowly increased. The ethylene oxide concentration in the tail gas will rise synchronously.

8. The acclimation method according to claim 1, characterized in that: In percentage by weight, the composition of the ethylene epoxide silver catalyst comprises: Silver: 21-33%; One or more alkali metals: 0-0.3%; One or more alkaline earth metals: 0-0.3%; One or more metals of Group VIIB: 0-0.31%; Aluminum oxide: 67-79%.