Mould shell for preparing alloy target ring, alloy target ring and preparation method of alloy target ring
By combining zircon powder and mullite powder mold shells with insulation cotton wrapping and vacuum induction furnace casting methods, the problems of alloy target ring mold shell strength and ingot cracking are solved, and the compactness and composition uniformity of the MCrAlY alloy target ring are achieved, simplifying The preparation process is simplified and is suitable for the preparation of highly brittle alloy target rings for vacuum arc plating deposition of thermal barrier coatings.
Patent Information
- Application Number
- CN202410819028.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
AI Technical Summary
When preparing alloy target rings, the existing technology has problems such as low mold shell strength, easy liquid leakage and ingot cracking during casting, and the process is complex, making it difficult to effectively improve the brittleness and composition uniformity of MCrAlY alloy.
Using a mold shell composed of zircon powder and mullite powder, through the design of the feeding opening mold shell and annular mold shell, combined with the low-temperature wax preparation process and the vacuum induction furnace casting method, the insulation cotton wrapping and slow cooling treatment are used to slow down the solidification process. Thermal stress to avoid ingot cracking, and the thermal barrier coating is prepared by vacuum arc plating deposition.
It achieves the compactness and composition uniformity of the alloy target ring, simplifies the preparation process, and improves the structural density and performance of the MCrAlY alloy target ring. It is suitable for direct molding of highly brittle alloys and is used for vacuum arc plating deposition to prepare thermal barrier coatings.
Smart Images

Figure CN118720053A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of alloy precision casting, and in particular to a mold shell for preparing an alloy target ring, an alloy target ring and a preparation method thereof. Background Art
[0002] Thermal barrier coating technology is widely used in high temperature protection of turbine blades of gas turbines and aircraft engines. The thermal barrier coating is composed of an intermediate MCrAlY metal bonding layer and an outer ceramic insulation layer. Among them, the MCrAlY coating is a bonding layer between the ceramic layer and the base alloy. It can improve the oxidation resistance and corrosion resistance of the base high-temperature alloy and the bonding strength of the ceramic layer. Its thermal expansion coefficient and other properties directly determine the service performance and life of the thermal barrier coating system. With the increase of fuel ratio, thrust-to-weight ratio or flow ratio, the operating temperature of the hot end component turbine blades continues to increase. The development of a MCrAlY bonding layer alloy system with a longer service life is a focus of attention at home and abroad.
[0003] However, the current mold shell for preparing alloy target rings, alloy target rings and preparation methods thereof still need to be improved. Summary of the invention
[0004] The embodiments of the present disclosure provide a mold shell for preparing an alloy target ring, an alloy target ring and a preparation method thereof, so as to solve or alleviate one or more technical problems in the related art.
[0005] As a first aspect of an embodiment of the present disclosure, an embodiment of the present disclosure provides a mold shell for preparing an alloy target ring, the mold shell comprising: a surface layer and a back layer arranged in sequence from the inside to the outside, the material forming the surface layer comprises zircon powder, and the thickness of the surface layer is 0.6-1.2 mm; the material forming the back layer comprises mullite powder, and the thickness of the back layer is 3.8-7 mm; the mold shell further comprises a shrinkage-filling mold shell and an annular mold shell connected to the shrinkage-filling mold shell, the thickness of the annular mold shell is 5-8 mm, and the thickness of the shrinkage-filling mold shell is 2-3.8 mm thicker than the thickness of the annular mold shell.
[0006] In a possible embodiment, the mesh number of the zircon powder forming the surface layer is 80-100 mesh, and the mold shell further includes a surface layer sealing layer, which is arranged between the surface layer and the back layer, and the material forming the surface layer sealing layer includes zircon powder slurry; the back layer includes a first back layer and a second back layer arranged in sequence, the first back layer is arranged close to the surface layer, the first back layer includes 2 stacked layers of mullite powder with a mesh number of 30-60 mesh, and the thickness of the first back layer is 1-2mm; the second back layer includes 4 stacked layers of mullite powder with a mesh number of 16-30 mesh, and the thickness of the second back layer is 2.8-5mm.
[0007] In a possible implementation, the mold shell further includes: a sealing layer, wherein the sealing layer is arranged on a side of the back layer away from the surface layer, and the material forming the sealing layer includes mullite slurry.
[0008] As a second aspect of an embodiment of the present disclosure, an embodiment of the present disclosure provides a method for preparing an alloy target ring, the method comprising: preparing a mold shell as described in any of the foregoing items by adopting a low-temperature wax preparation process; wrapping thermal insulation cotton on the outside of the mold shell, wherein the thickness of the thermal insulation cotton wrapped on the outside of the shrinkage-filling mold shell is greater than the thickness of the thermal insulation cotton wrapped on the outside of the annular mold shell; and baking the wrapped mold shell; smelting metal raw materials in a vacuum induction furnace to form an alloy melt; vacuum casting the alloy melt using the mold shell, and cooling it in a vacuum environment after casting to form an alloy target ring blank; processing and forming the alloy target ring blank to form the alloy target ring.
[0009] In a possible embodiment, the thickness of the thermal insulation cotton is 10-15 mm, and two layers of the thermal insulation cotton are wrapped around the shrinkage-filling mold shell and the annular mold shell 8-12 cm near one end of the shrinkage-filling mold shell; one layer of the thermal insulation cotton is wrapped around the outside of the annular mold shell; the temperature of the baked treatment of the wrapped mold shell is 1050-1200°C, and the baking time is 3-5 hours.
[0010] In a possible implementation, a first metal is first added to the vacuum induction furnace, and then the second metal is added, wherein the oxidation activity of the first metal is lower than that of the second metal; the purity of the metal raw material used for the smelting is 99.9-99.98%; after the first metal is added, the first melting vacuum degree in the vacuum induction furnace is 0.2-1Pa, and the first melting temperature is 1530-1560°C; after the first metal is completely melted, the second metal is added, and after the second metal is added, the second melting vacuum degree in the vacuum induction furnace is 0.2-1Pa, the second melting temperature is 1580-1650°C, and the second melting time is 10-15min.
[0011] In a possible implementation, during the vacuum casting, the temperature of the alloy melt is 1480-1520°C; the vacuum casting time is 3-5s; the cooling treatment time is 8-10h, and the alloy is cooled to 200-300°C to form the alloy target ring rough blank.
[0012] In a possible embodiment, the processing and forming process includes: cutting the alloy target ring rough blank, removing the shrinkage feeder, and using wire cutting to remove 2-3 mm on each side of the inner and outer circular surfaces, and then using a grinder to obtain the alloy target ring, wherein the impurity content in the alloy target ring is less than 0.7wt%.
[0013] In a possible embodiment, the method includes: the first metal added to the vacuum induction furnace includes: Ni block, Co block, Cr particles, and the second metal added includes cylindrical rod-shaped Al, Al skin-wrapped Y block, and Al skin-wrapped Re block; the first melting vacuum degree is 1Pa, the first melting temperature is 1560°C, and after the first metal is completely melted, argon gas is filled to 6kPa, the cylindrical rod-shaped Al is first added, and after the cylindrical rod-shaped Al is completely melted, the Al skin-wrapped Y block and the Al skin-wrapped Re block are added; vacuuming to 0.5Pa again, the second melting vacuum degree is 0.5Pa, the second melting temperature is 1620°C, and the second melting time is 15min; then the temperature is reduced to 1500°C and maintained at the temperature degree; after the vacuum casting treatment is completed, the alloy target ring blank is cooled to 250°C under a vacuum degree of 1-5Pa for 10 hours to obtain the alloy target ring blank, which is an MCrAlY alloy target ring blank, and the composition of the MCrAlY alloy target ring blank is Ni32.1wt%, Co27.8wt%, Cr17.3wt%, Al17.4wt%, Y0.71wt%, and Re4.7wt%; the alloy target ring blank is machined, the feeding cap is cut off by wire cutting, 2.5mm of each side of the inner circle surface and the outer circle surface are cut off, and then polished by a grinder to obtain the alloy target ring, which is an MCrAlY alloy target ring, and the dimensions of the alloy target ring are an outer diameter of 150mm, an inner diameter of 130mm, and a height of 120mm.
[0014] As a second aspect of an embodiment of the present disclosure, an embodiment of the present disclosure provides an alloy target ring, which is prepared by any of the methods described above, and the alloy target ring can be used as a bonding layer for preparing a thermal barrier coating by vacuum arc plating deposition. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments according to the present disclosure and should not be regarded as limiting the scope of the present disclosure.
[0016] Figure 1 It is a schematic diagram of a method for preparing an alloy target ring according to one embodiment of the present disclosure;
[0017] Figure 2 A schematic diagram of a partial method for preparing an alloy target ring according to an embodiment of the present disclosure;
[0018] Figure 3 This is a picture of an alloy target ring blank prepared according to a method according to an embodiment of the present disclosure;
[0019] Figure 4 This is a top surface picture of an alloy target ring prepared according to a method according to an embodiment of the present disclosure;
[0020] Figure 5 This is a side view of an alloy target ring prepared according to a method according to an embodiment of the present disclosure;
[0021] Figure 6 The figure is a picture of an alloy target ring blank prepared according to a comparative example of the present disclosure.
[0022] Description of reference numerals:
[0023] 1: pouring cup; 2: thermal insulation cotton; 3: mold runner; 4: shrinkage feed riser; 5: ring mold. DETAILED DESCRIPTION
[0024] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present disclosure, and different embodiments may be combined arbitrarily without conflict. Therefore, the drawings and descriptions are considered to be illustrative in nature and not restrictive.
[0025] As a first aspect of an embodiment of the present disclosure, an embodiment of the present disclosure provides a mold shell for preparing an alloy target ring, the mold shell comprising: a surface layer and a back layer arranged in sequence from the inside to the outside, the material forming the surface layer comprises zircon powder, the material forming the back layer comprises mullite powder, and the thickness of the surface layer is 0.6-1.2mm; the material forming the back layer comprises mullite powder, and the thickness of the back layer is 3.8-7mm; specifically, the mold shell further comprises a shrinkage-filling mold shell and an annular mold shell connected to the shrinkage-filling mold shell, the thickness of the annular mold shell is 5-8mm, and the thickness of the shrinkage-filling mold shell is 2-3.8mm thicker than the thickness of the annular mold shell. Therefore, by making the thickness of the shrinkage-supporting mold shell thicker than the thickness of the lower annular mold shell, the mold shell can slow down the solidification process when casting the alloy using the mold shell, and can effectively avoid the cracking of the ingot caused by thermal stress during the solidification process. The mold shell is particularly suitable for the direct forming of high-brittle alloy target rings, such as the direct forming of high-brittle MCrAlY alloy target rings. The alloy target ring prepared using the mold shell has good structural density, uniform composition, and a simple preparation process.
[0026] It should be noted that the thickness of the annular mold shell mentioned above may include the total thickness of the surface layer and the back layer in the annular mold shell; the thickness of the feeding mold shell mentioned above may include the total thickness of the surface layer and the back layer in the feeding mold shell.
[0027] For ease of understanding, the principle by which the mold shell according to the embodiment of the present application can achieve the above-mentioned beneficial effects is described in detail below: The inventors have found that in the field of thermal barrier coating preparation, in the prior art, in order to prepare a high-temperature oxidation-resistant low-expansion bonding layer alloy component system, the technical idea is to increase the content of the low-expansion β-NiAl phase in the MCrAlY alloy to effectively reduce the expansion coefficient of the alloy while improving the oxidation resistance. However, the excessive content of the β-NiAl phase leads to a serious increase in the brittleness of the target material. In order to solve the problem of high machining difficulty caused by the high brittleness and high hardness of the MCrAlY alloy, such alloys can be prepared by a powder metallurgy method of pre-alloying and then mixed powder sintering. However, powder materials are required in the powder metallurgy process, which is not as demanding as the smelting method. In addition, the powder metallurgy ball milling process increases the risk of oxidation, and the high sintering pressure increases the risk factor. Some technologies use vacuum induction furnace melting combined with Al 2 O 3 -SiO 2 The alloy is prepared by combining mold shell casting, but Al 2 O 3 -SiO 2 The low strength of the mold shell is prone to leakage during pouring. The multi-principal alloy target materials involved in some technologies use a two-step method of vacuum induction furnace melting to prepare the master alloy + vacuum precision casting to prepare the alloy cylindrical target ingot cracking, but the process is relatively long and the steps are relatively complicated.
[0028] In view of the shortcomings of the prior art, the present invention provides a mold shell for preparing an alloy target ring. In order to avoid the cracking of the ingot caused by the thermal stress during the solidification process of the target ring, a mold shell with a surface layer of zircon sand and a back layer of mullite is used, and the thickness of the shrinkage-filling mold shell is thicker than the thickness of the lower annular mold shell, so that the solidification process when the alloy is cast using the mold shell can be slowed down, and the cracking of the ingot caused by the thermal stress during the solidification process can be effectively avoided. The mold shell is particularly suitable for the direct forming of high-brittle alloy target rings, such as the direct forming of high-brittle MCrAlY alloy target rings. The alloy target ring prepared using the mold shell has good structural density, uniform composition, and a simple preparation process. And when the mold shell is used to prepare the alloy target ring in the future, it is combined with a suitable cotton packing process and vacuum long-term slow cooling to further solve the problem of easy cracking of the high-brittle target material. The preparation process is simple, and the obtained alloy target material has good structural density and uniform composition.
[0029] In a possible embodiment, the thickness of the surface layer may be 0.6-1.2 mm, for example, 0.6-1.2 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, etc.; in a possible embodiment, the mesh size of the zircon powder forming the surface layer may be 80-100 mesh, for example, 85 mesh, 90 mesh, 95 mesh, etc.; specifically, the mold shell may further include a surface layer sealing layer, the surface layer sealing layer is arranged between the surface layer and the back layer, and the material forming the surface layer sealing layer may include zircon powder slurry.
[0030] In a possible embodiment, the back layer may include a first back layer and a second back layer arranged in sequence, the first back layer is arranged close to the surface layer, and the first back layer may include 2 layers of stacked mullite powder with a mesh number of 30-60 meshes; specifically, the mesh number of the mullite powder in the first back layer may be 30-45 meshes, for example, 35 meshes, 40 meshes, 43 meshes, etc.; specifically, the thickness of the first back layer may be 1-2mm, 1-1.2mm, 1.3mm, 1.5mm, 1.7mm, 1.9mm, etc. Specifically, the second back layer may include 4 layers of stacked mullite powder with a mesh number of 16-30 meshes, for example, 16-22 meshes, 20 meshes, 25 meshes, etc.; specifically, the thickness of the second back layer may be 2.8-5mm, 2.8-3.5mm, 3mm, 3.5mm, 4mm, 4.5mm, etc.
[0031] In a possible embodiment, the total thickness of the annular mold shell can be 5-8mm, for example, it can be 5.2mm, 5.5mm, 5.7mm, 6mm, 6.5mm, 7mm, 7.5mm, etc.; specifically, the thickness of the shrinkage-filling mold shell can be 2-3.8mm thicker than the thickness of the annular mold shell, for example, it can be 2-3mm thick, and can be 2.2mm, 2.5mm, 2.7mm, 3mm, 3.2mm, 3.5mm, 3.6mm, etc.
[0032] In a possible implementation, the mold shell further includes: a sealing layer, which is arranged on a side of the back layer away from the surface layer, and the material forming the sealing layer may include mullite slurry.
[0033] As a second aspect of the embodiment of the present disclosure, the embodiment of the present disclosure provides a method for preparing an alloy target ring, in which the mold shell is designed so that the thickness of the supplementary mold shell is thicker than the thickness of the lower annular mold shell, so that the solidification process when the alloy is cast using the mold shell can be slowed down, and the cracking of the ingot caused by thermal stress during the solidification process can be effectively avoided. The alloy target ring prepared using the mold shell has good structural density, uniform composition, and a simple preparation process; and the method solves the problem of easy cracking of the high-brittle target ring by wrapping thermal cotton on the outside of the mold shell, and making the thickness of the thermal cotton wrapped on the outside of the supplementary mold shell greater than the thickness of the thermal cotton wrapped on the outside of the annular mold shell, and slowly cooling for a long time in a vacuum environment, so that the preparation process is simple, and the obtained alloy target ring has good structural density and uniform composition. The method is particularly suitable for preparing a high-brittle MCrAlY alloy target ring, which is used as a bonding layer for preparing thermal barrier coatings by vacuum arc plating deposition, and has good performance. That is to say, the method for preparing a high-brittle alloy target ring provided in the present application uses a mold shell with a surface layer of zircon sand and a back layer of mullite sand, assisted by a suitable cotton wrapping process and slow cooling under vacuum, and a one-step vacuum induction melting and casting method to prepare a high-brittle MCrAlY ring target material for vacuum arc plating. The preparation process is simpler and easy to operate, and the prepared target material has a dense composition and meets the requirements of the vacuum arc plating method.
[0034] In one possible implementation, reference Figure 1 , the method comprising:
[0035] S100: Making the mold shell
[0036] In this step, the mold shell described above is prepared by a low-temperature wax preparation process, so this method has all the characteristics and beneficial effects of the mold shell described above, which will not be repeated here.
[0037] S200: Wrap the outer side of the mold with insulation cotton and bake it
[0038] In this step, the outer side of the mold shell prepared in the previous step is wrapped with thermal insulation cotton, wherein the thickness of the thermal insulation cotton wrapped on the outer side of the shrinkage-filling mold shell is greater than the thickness of the thermal insulation cotton wrapped on the outer side of the annular mold shell. Thus, the solidification process when the alloy is cast using the mold shell can be slowed down, and the cracking of the ingot caused by thermal stress during the solidification process can be effectively avoided. The alloy target ring prepared by this method has good structural density, uniform composition, and a simple preparation process. In a possible embodiment, the thickness of the thermal insulation cotton is 10-15mm, for example, 13mm, and 2 layers of thermal insulation cotton are coated on the shrinkage-filling mold shell and the annular mold shell 8-12cm close to one end of the shrinkage-filling mold shell; and 1 layer of thermal insulation cotton is wrapped on the outer side of the annular mold shell. Specifically, refer to Figure 2 ( Figure 2The pouring cup mouth 1 is shown in the figure, the mold shell runner 3, the shrinkage feeding riser 4 and the lower edge 10mm are wrapped with 2 layers of 13mm thick insulation cotton 2, each layer of insulation cotton 2 is fixed with iron wire to fit the mold shell tightly; the lower part of the remaining annular mold shell 5 is wrapped with 1 layer of 13mm thick insulation cotton 2. In a possible embodiment, the wrapped mold shell is baked, and the baking temperature can be 1050-1200℃, and the baking time can be 3-5 hours. Specifically, the mold shell can be baked in a muffle furnace to 1050-1200℃, and the baking time is 3-5 hours.
[0039] S300: Melting metal raw materials into alloy melt in a vacuum induction furnace
[0040] In this step, the metal raw material is melted in a vacuum induction furnace to form an alloy melt. In a possible embodiment, the first metal is first added to the vacuum induction furnace, and then the second metal is added, wherein the oxidation activity of the first metal is lower than the oxidation activity of the second metal. Specifically, the purity of the metal raw material used for smelting is 99.9-99.98%. Specifically, after adding the first metal, the first melting vacuum degree in the vacuum induction furnace can be 0.2-1Pa, and the first melting temperature can be 1530-1560°C; after the first metal is completely melted, the second metal is added, and after adding the second metal, the second melting vacuum degree in the vacuum induction furnace can be 0.2-1Pa, the second melting temperature can be 1580-1650°C, and the second melting time can be 10-15min.
[0041] In a possible embodiment, the first metal added to the vacuum induction furnace includes: Ni block, Co block, Cr particles, and the second metal added includes cylindrical rod-shaped Al, Al skin-wrapped Y block, and Al skin-wrapped Re block; the first melting vacuum degree is 1Pa, the first melting temperature is 1560°C, and after the first metal is completely melted, argon gas is filled to 6kPa, and cylindrical rod-shaped Al is added first. After Al is completely melted, the Al skin-wrapped Y block and the Al skin-wrapped Re block are added; the vacuum is evacuated to 0.5Pa again, the second melting vacuum degree is 0.5Pa, the second melting temperature is 1620°C, and the second melting time is 15min; then the temperature is reduced to 1500°C and the temperature is maintained.
[0042] Specifically, when adding metals to a vacuum induction furnace, those with low oxidation activity, such as Ni, Co, and Cr, are directly loaded into the crucible with the furnace, and those with higher oxidation activity, such as Al, Y, and Re, are added in batches. In the presence of multiple active elements, Al is added first, and then other active metals are added. Specifically, Ni and Co are in the form of 5-10 mm blocks, Cr is in the form of granules, Al is in the form of cylindrical short rods, Y is in the form of large particles, and Re is in the form of granules. Y and Re are added by wrapping Al skin. Specifically, the added metals with higher oxidation activity may also include Hf, which may be in the form of granules or wrapped in Al skin. Specifically, the alloy smelting is carried out in a medium-frequency vacuum induction melting furnace. The vacuum degree of the initial melting process is 0.2-1Pa. After the charge at 1530-1560°C is completely melted, the active metal is added for the second time. Before adding Al, high-purity argon is filled to 5-10kPa to prevent the melt from overcooling and splashing. After Al is melted, other active metals 0.5-1%wt% Y, 0.5-3wt% Hf, 1-7wt% Re are added. Then the vacuum is controlled to 0.2-1Pa and the temperature is 1580-1650℃ for refining for 10-15min. Specifically, high-purity argon is filled to 8-10kPa before adding aluminum, and the refining temperature is 1620-1650℃.
[0043] S400: Use the mold shell to vacuum cast the alloy melt to form the alloy target ring rough blank
[0044] In this step, the alloy melt formed by smelting in the previous step is vacuum cast using the mold shell prepared in the previous step, and after casting, it is cooled in a vacuum environment to form a rough alloy target ring. In one possible embodiment, during vacuum casting, the temperature of the alloy melt can be 1480-1520°C; the vacuum casting time is 3-5s, the cooling time is 8-10h, cooled to 200-300°C, taken out of the furnace and broken into a shell, to form a rough alloy target ring. In this method, the cooling time is slow, and slow cooling can effectively avoid cracking of the ingot caused by thermal stress during the solidification process. The alloy target ring prepared by this method has good structural density, uniform composition, and a simple preparation process.
[0045] In a possible embodiment, after the vacuum casting treatment is completed, it can be cooled to 250°C for 10 hours under a vacuum degree of 1-5Pa to obtain an alloy target ring rough blank. The prepared alloy target ring rough blank is an MCrAlY alloy target ring rough blank. The composition of the MCrAlY alloy target ring rough blank can be Ni32.1wt%, Co27.8wt%, Cr17.3wt%, Al17.4wt%, Y0.71wt%, and Re4.7wt%.
[0046] S500: Processing and forming the alloy target ring blank to form the alloy target ring
[0047] In this step, the rough alloy target ring is processed and formed to form the alloy target ring. In a possible implementation, the processing and forming includes: cutting the rough alloy target ring, cutting off the feeding riser, and cutting off the inner and outer surfaces by 2-3 mm on each side by wire cutting, and then processing the alloy target ring by a grinder, wherein the impurity content in the alloy target ring is less than 0.7 wt%. Specifically, the inner and outer surfaces can be processed by 2-2.5 mm on each side, and the impurity content of the target material can be less than 0.4 wt%.
[0048] In a possible implementation, the alloy target ring blank prepared in the previous step is rough-machined, the feeding cap opening is cut off by wire cutting, the inner and outer circular surfaces are cut off by 2.5 mm each, and then ground by a grinder to obtain an alloy target ring, which is an MCrAlY alloy target ring, and the dimensions of the alloy target ring are an outer diameter of 150 mm, an inner diameter of 130 mm, and a height of 120 mm.
[0049] As a third aspect of the embodiment of the present disclosure, the embodiment of the present disclosure provides an alloy target ring, which is prepared by the method described above, and the alloy target ring can be used as a bonding layer for preparing a thermal barrier coating by vacuum arc plating deposition. Therefore, the alloy target ring has all the characteristics and advantages of the alloy target ring prepared by the method described above, and the alloy target ring has a simple preparation process, good tissue density, uniform composition, and good performance.
[0050] Embodiment 1:
[0051] The composition of the smelted high brittle MCrAlY alloy is Ni32.1wt%, Co27.8wt%, Cr17.3wt%, Al17.4wt%, Y0.71wt%, Re4.7wt%;
[0052] Place Ni blocks, Co blocks, and Cr particles in the crucible of a vacuum induction melting furnace, add cylindrical aluminum rods into the secondary charging bin, and wrap Y blocks and Re blocks with Al skins and add them into the secondary charging shovel. Evacuate to 1Pa and heat to melt. After the charge in the crucible at 1560℃ is completely melted, fill with argon to 6kPa, add Al rods for the second time, and after Al is completely melted, add Y and Re through the shovel. Evacuate to 0.5Pa again, increase the power, and heat to 1620℃ for refining for 15 minutes. After refining, cool to 1500℃ and maintain the temperature;
[0053] The mold runner, feeding riser and 10mm below the bottom edge are wrapped with 2 layers of 13mm thick insulation cotton, and the remaining lower part of the target ring is wrapped with 1 layer of 13mm thick insulation cotton. The mold wrapped with insulation cotton is baked at 1050℃ for 3 hours, and when the vacuum smelting is completed, it is quickly transferred to the vacuum casting chamber and evacuated to 1Pa. After the casting is completed, it is cooled for 10 hours to 250℃ under a vacuum degree of 1-5Pa, and then taken out of the furnace;
[0054] The obtained MCrAlY alloy target ingot is machined, the cap opening is cut off by wire cutting, the inner and outer surfaces are cut off by 2.5 mm each on one side, and the surface is polished by a grinder to obtain an MCrAlY alloy target ring with an outer diameter of 150 mm, an inner diameter of 130 mm, and a height of 120 mm;
[0055] The high brittle MCrAlY alloy target ring ingot cast in this embodiment has no thermal crack defects in appearance, no shrinkage holes or looseness on the upper part of the target ring, and the surface quality of the target ring is good. Figure 3-5 shown.
[0056] Comparative Example 1
[0057] Compared with Example 1, the mold shell materials used are the same, the surface layer is zircon sand, and the back layer is mullite. No cotton packing and slow cooling under vacuum are performed, and as a result, obvious cracks appear in the ring casting. Figure 6 shown.
[0058] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present disclosure, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0059] In the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.
[0060] In the present disclosure, unless otherwise clearly specified and limited, the first feature "above" or "below" the second feature may include the first and second features being in direct contact, or the first and second features being not in direct contact but in contact through another feature between them. Moreover, the first feature "above", "above" and "above" the second feature include the first feature being directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. The first feature "below", "below" and "below" the second feature include the first feature being directly above and obliquely above the second feature, or simply indicates that the first feature is lower in level than the second feature. The above disclosure provides many different embodiments or examples for implementing different structures of the present disclosure. In order to simplify the present disclosure, the components and settings of specific examples are described above. Of course, they are merely examples and are not intended to limit the present disclosure. In addition, the present disclosure may repeat reference numbers and / or reference letters in different examples, and such repetition is for the purpose of simplification and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed.
[0061] The above are only specific embodiments of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.
Claims
1. A mold shell for preparing an alloy target ring, characterized in that: include: A surface layer and a back layer are sequentially arranged from the inside to the outside, wherein the material forming the surface layer includes zircon powder, and the thickness of the surface layer is 0.6-1.2 mm; The material forming the back layer includes mullite powder, and the thickness of the back layer is 3.8-7mm; the mold shell further includes a shrinkage-filling mold shell and an annular mold shell connected to the shrinkage-filling mold shell, the thickness of the annular mold shell is 5-8mm, and the thickness of the shrinkage-filling mold shell is 2-3.8mm thicker than the thickness of the annular mold shell.
2. The formwork according to claim 1, characterized in that: The mesh number of the zircon powder forming the surface layer is 80-100 meshes, and the mold shell further includes a surface layer sealing layer, which is arranged between the surface layer and the back layer, and the material forming the surface layer sealing layer includes zircon powder slurry; the back layer includes a first back layer and a second back layer arranged in sequence, the first back layer is arranged close to the surface layer, the first back layer includes 2 stacked layers of mullite powder with a mesh number of 30-60 meshes, and the thickness of the first back layer is 1-2mm; the second back layer includes 4 stacked layers of mullite powder with a mesh number of 16-30 meshes, and the thickness of the second back layer is 2.8-5mm.
3. The formwork according to claim 1, characterized in that: Further including: The sealing layer is arranged on a side of the back layer away from the surface layer, and the material forming the sealing layer includes mullite slurry.
4. A method for preparing an alloy target ring, characterized in that: include: The mold shell according to any one of claims 1 to 3 is prepared by a low-temperature wax preparation process; Wrapping the outer side of the mold shell with thermal insulation cotton, wherein the thickness of the thermal insulation cotton wrapped on the outer side of the shrinkage-filling mold shell is greater than the thickness of the thermal insulation cotton wrapped on the outer side of the annular mold shell; and baking the wrapped mold shell; The metal raw materials are melted in a vacuum induction furnace to form an alloy melt; The alloy melt is vacuum-casted by using the mold shell, and after casting, it is cooled in a vacuum environment to form a rough alloy target ring; The alloy target ring blank is processed and formed to form the alloy target ring.
5. The method according to claim 4, characterized in that The thickness of the thermal insulation cotton is 10-15mm, and two layers of the thermal insulation cotton are wrapped around the shrinkage-filling mold shell and the annular mold shell 8-12cm away from one end of the shrinkage-filling mold shell; one layer of the thermal insulation cotton is wrapped around the outside of the annular mold shell; the temperature for the baking treatment of the wrapped mold shell is 1050-1200°C, and the baking time is 3-5 hours.
6. The method according to claim 4, characterized in that A first metal is first added to the vacuum induction furnace, and then the second metal is added, wherein the oxidation activity of the first metal is lower than that of the second metal; the purity of the metal raw material used in the smelting is 99.9-99.98%; after the first metal is added, the first melting vacuum degree in the vacuum induction furnace is 0.2-1Pa, and the first melting temperature is 1530-1560°C; after the first metal is completely melted, the second metal is added, and after the second metal is added, the second melting vacuum degree in the vacuum induction furnace is 0.2-1Pa, the second melting temperature is 1580-1650°C, and the second melting time is 10-15min.
7. The method according to claim 4, characterized in that During the vacuum casting, the temperature of the alloy melt is 1480-1520° C.; the vacuum casting time is 3-5 seconds; the cooling treatment time is 8-10 hours, and the alloy is cooled to 200-300° C. to form the alloy target ring rough blank.
8. The method according to claim 4, characterized in that The processing and forming process includes: The alloy target ring blank is cut to remove the shrinkage feeder, and the inner and outer surfaces are cut by wire cutting by 2-3 mm each on one side, and then the alloy target ring is obtained by grinding. The impurity content in the alloy target ring is less than 0.7wt%.
9. The method according to claim 6, characterized in that include: The first metal added to the vacuum induction furnace includes: Ni block, Co block, Cr particles, and the second metal added includes cylindrical rod-shaped Al, Al skin-wrapped Y block, and Al skin-wrapped Re block; the first melting vacuum degree is 1Pa, the first melting temperature is 1560°C, and after the first metal is completely melted, argon gas is filled to 6kPa, and the cylindrical rod-shaped Al is first added. After the cylindrical rod-shaped Al is completely melted, the Al skin-wrapped Y block and the Al skin-wrapped Re block are added; the vacuum is evacuated to 0.5Pa again, the second melting vacuum degree is 0.5Pa, the second melting temperature is 1620°C, and the second melting time is 15min; the temperature is then reduced to 1500°C and maintained at the temperature; After the vacuum casting process is completed, the alloy target ring blank is cooled to 250° C. at a vacuum degree of 1-5 Pa for 10 hours to obtain the alloy target ring blank, wherein the alloy target ring blank is an MCrAlY alloy target ring blank, and the composition of the MCrAlY alloy target ring blank is Ni32.1wt%, Co27.8wt%, Cr17.3wt%, Al17.4wt%, Y0.71wt%, and Re4.7wt%; The alloy target ring blank is machined, the feeding cap opening is cut off by wire cutting, 2.5 mm is cut off on one side of the inner circle surface and the outer circle surface, and then ground by a grinder to obtain the alloy target ring. The alloy target ring is an MCrAlY alloy target ring, and the dimensions of the alloy target ring are an outer diameter of 150 mm, an inner diameter of 130 mm, and a height of 120 mm.
10. An alloy target ring, characterized in that: The alloy target ring is prepared by the method described in any one of claims 4 to 9, and the alloy target ring can be used as a bonding layer for preparing thermal barrier coatings by vacuum arc plating deposition.