Submersed nozzle and method for improving quality of casting blank

By designing an immersed nozzle with an upper outlet and a lower outlet and an argon blowing system, the flow rate of molten steel flowing through the mold is adjusted, which solves the problems of slag entrainment and liquid level fluctuations in the continuous steel casting process, and significantly improves the quality and quality of the slab. Melting efficiency.

CN118720121AActive Publication Date: 2024-10-01ANGANG STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411059886.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

In the continuous steel casting process, the slag entrainment problem caused by the vortex of the molten steel level in the mold leads to the formation of inclusions in the cast slab. It is difficult to effectively solve it with the existing technology, and the liquid level fluctuation caused by unstable injection flow affects the casting process. Blank quality.

Method used

Design an immersed nozzle including an upper outlet and a lower outlet, combined with an argon blowing system, to control the flow of molten steel through the mold by adjusting the argon gas flow, reduce liquid level fluctuations and slag entrainment, and ensure the quality of the cast slab.

Benefits of technology

It significantly reduces inclusions and longitudinal crack defects in the slab, improves the overall quality of the slab, reduces the liquid surface temperature, and enhances the melting effect of the mold slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720121A_ABST
    Figure CN118720121A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of submersed nozzles, in particular to a submersed nozzle and a method for improving casting blank quality. Comprising a submersed nozzle and an argon blowing system, the body of the submersed nozzle is a long cylinder with an open top end and a closed bottom end; an upper outlet and a lower outlet are formed in the lower part of the body; the upper outlet inclines upwards, the lower outlet inclines downwards, and the upper outlet is located above the lower outlet; the argon blowing system comprises a gas inlet pipe, a lower through pipe and a gas outlet pipe; the gas inlet pipe is connected with an argon pipeline and extends into the upper part of the side wall of the body, the lower through pipe is vertically arranged on the side wall of the body, the top of the lower through pipe is communicated with the gas inlet pipe, the bottom of the lower through pipe is positioned at the upper outlet, and the bottom of the lower through pipe is communicated with the gas outlet pipe; argon enters from the gas inlet pipe, passes through the lower through pipe and is sprayed out from the gas outlet pipe. And the casting blank quality can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of submerged nozzles, and in particular to a submerged nozzle and a method for improving the quality of a casting. Background Art

[0002] During the continuous steel casting process, vortices often form on the surface of the molten steel in the crystallizer, which draws the protective slag covering the liquid surface into the molten steel. This is called "eddy slag entanglement". The entrained protective slag is retained in the ingot to form large-particle inclusions, leading to various inclusion defects in the rolled material, such as surface defects of thin plates for automobile panels, flaw detection defects of thick plate steel for shipbuilding, bridges and containers, etc., resulting in the scrapping of steel and causing significant economic losses.

[0003] The "slag entanglement" problem can currently only be controlled by adjusting the outlet angle of the submerged nozzle, blowing argon gas volume, stabilizing the steel casting flux, etc., but the effect is not ideal. It can be said that there is no very effective way to solve the "slag entanglement" problem. In addition, the liquid level fluctuation caused by unstable injection flow will lead to slag inclusion defects on the surface of the billet. In addition, the impact of the stream on the billet shell causes uneven thickness of the billet shell, resulting in defects such as longitudinal cracks in the billet.

[0004] The Chinese patent document with the publication number CN201644781U discloses "a crystallizer submerged nozzle for preventing slag rolling in continuous casting slabs". Although it overcomes the large liquid level fluctuation and excessive surface flow rate caused by the unreasonable size and hole type of the crystallizer submerged nozzle during continuous casting, effectively prevents the entanglement of protective slag, and reduces the defects such as slag rolling and slag inclusion on the surface of the casting slab; however, there is a problem that the molten steel flow flowing out of the submerged nozzle impacts too much downward, resulting in a low temperature of the molten steel surface in the crystallizer, making the protective slag in the crystallizer poorly melted, affecting the quality of the continuous casting slab. The Chinese patent document with the publication number CN101219464 discloses "a continuous casting crystallizer device capable of controlling the liquid surface flow field and fluctuation". Although it can reduce and inhibit the generation of slag rolling in the crystallizer, thereby improving the quality of the continuous casting slab; however, it has the problem that the protective slag will be brought into the molten steel when the metal plate is consumed, and the flow of the protective slag is hindered. In addition, its structure is complicated, which increases the difficulty of operation and production cost, and cannot meet the needs well. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the present invention provides an immersed nozzle and method for improving the quality of the casting, which can significantly improve the quality of the casting.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A submerged nozzle for improving the quality of ingot castings comprises a submerged nozzle and an argon blowing system; the body of the submerged nozzle is a long tube with an open top and a closed bottom; an upper outlet and a lower outlet are arranged at the lower part of the body; the upper outlet is inclined upward, the lower outlet is inclined downward, and the upper outlet is located above the lower outlet; the argon blowing system comprises an air inlet pipe, a down pipe and an air outlet pipe; the air inlet pipe is connected to an argon gas pipeline, the air inlet pipe extends into the upper part of the side wall of the body, the down pipe is vertically arranged on the side wall of the body, the top of the down pipe is connected to the air inlet pipe, the bottom of the down pipe is located at the upper outlet, and the bottom of the down pipe is connected to the air outlet pipe; argon gas enters from the air inlet pipe, passes through the down pipe, and is ejected from the air outlet pipe.

[0008] Furthermore, the angle between the upper outlet and the axis of the body is α, 50°≤α≤80°;

[0009] Furthermore, the angle between the lower outlet and the axis of the body is β, 55°≤β≤85°.

[0010] Furthermore, the distance between the upper outlet and the lower outlet is S, 50mm≤α≤150mm.

[0011] Furthermore, the upper outlet is composed of two holes that are symmetrical on the left and right.

[0012] Furthermore, the lower outlet is composed of two holes that are symmetrical on the left and right.

[0013] Furthermore, the submerged nozzle is installed on the tundish.

[0014] Furthermore, the upper portion of the body is trumpet-shaped, and the lower portion is straight-cylindrical.

[0015] A method for improving the quality of a casting is implemented based on the above-mentioned submerged nozzle for improving the quality of a casting, and specifically comprises the following steps:

[0016] 1) Bake the immersion nozzle before use;

[0017] 2) Install the submerged nozzle on the tundish, and connect the argon blowing system air inlet pipe to the argon gas pipeline;

[0018] 3) Before pouring, turn on the argon blowing system. Argon enters from the air inlet pipe, passes through the lower pipe, and is ejected from the air outlet pipe;

[0019] 4) Start pouring and adjust the argon flow rate according to the slag melting and the crystallizer liquid level fluctuation during the continuous casting process. When the crystallizer liquid level fluctuation is greater than ±5mm, increase the argon flow rate by 10% to 90%; conversely, when the melting of the protective slag at the crystallizer liquid level is more than 10% lower than the set value, reduce the argon flow rate by 10% to 90% until the continuous casting ends.

[0020] Compared with the prior art, the present invention has at least the following technical effects or advantages:

[0021] The outlet of the immersion water inlet of the present invention is composed of an upper outlet and a lower outlet. The outlet angle of the upper outlet is upward, and the molten steel flowing out of it flows through the steel liquid surface of the crystallizer and then goes down into the deep liquid phase hole; the outlet angle of the lower outlet is downward, and a small part of the molten steel flowing out of it flows to the billet shell, and most of it goes down directly into the deep liquid phase hole. Argon gas enters from the air inlet pipe, and is ejected from the air outlet pipe through the lower pipe, and argon gas is blown into the molten steel to form argon bubbles; its function is to adjust the flow rate of the molten steel flow flowing out of the upper outlet. The larger the argon blowing amount, the smaller the molten steel flow rate, and vice versa. In this way, the flow rate of the molten steel flow flowing through the steel liquid surface of the crystallizer can be adjusted, thereby adjusting the slag-melting speed of the protective slag, and reducing the liquid level fluctuation, thereby controlling the quality of the ingot.

[0022] ① The flow rate of the stream flowing through the liquid surface can be adjusted at any time, which is beneficial to the quality control of the ingot; ② The amount of "head-on collision" of the molten steel flow near the submerged nozzle will be greatly reduced, so the slag rolling phenomenon will be greatly reduced: the flow collision of the liquid surface near the nozzle will be reduced or even eliminated; ③ The molten steel flow flowing out of the upper outlet directly flows through the liquid surface and contacts with the protective slag, instead of first impacting the narrow edge of the ingot shell and then returning to the liquid surface as originally done, thereby reducing the chance of inclusions being captured by the solidification front of the ingot shell, thereby reducing the inclusion content of the ingot; ④ The molten steel flow flowing out of the upper outlet directly flows through the liquid surface to reach the liquid surface of the crystallizer, and the liquid flow will become stable, so the fluctuation amplitude of the crystallizer liquid surface will be significantly reduced, reducing the occurrence of slag inclusion in the ingot shell, and at the same time reducing the depth of the vibration mark; ⑤ The impact of the stream on the ingot shell is reduced, the uneven thickness of the ingot shell is improved, and the occurrence of defects such as longitudinal cracks is reduced; ⑥ The liquid surface temperature is higher, which is conducive to accelerating the melting of the protective slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the structure and process principle of the present invention.

[0024] Figure 2 yes Figure 1 A partial enlarged view of .

[0025] In the figure:

[0026] 1-body 2-inlet pipe 3-lower pipe 4-outlet pipe 5-upper outlet 6-lower outlet 7-crystallizer α-angle between upper outlet and body axis β-angle between lower outlet and body axis S-distance between upper outlet and lower outlet DETAILED DESCRIPTION

[0027] The embodiments of the present invention are described in detail below. In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described in combination with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0029] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0030] In the description of the present invention, it should be noted that the terms used herein are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0031] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, the numerical expressions and numerical values ​​do not limit the scope of the present invention. At the same time, it should be clear that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be regarded as part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings.

[0032] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0033] like Figure 1 , Figure 2 As shown, a submerged nozzle for improving the quality of the casting, including a submerged nozzle and an argon blowing system, wherein the submerged nozzle is installed on a tundish.

[0034] The main body of the immersion nozzle is arranged vertically, with a vertical axis, and is a long cylinder with an open top and a closed bottom. The upper part of the main body 1 is a trumpet-shaped cylinder, and the lower part is a straight cylinder.

[0035] The bottom of the body 1 is provided with an upper outlet 5 and a lower outlet 6, the upper outlet 5 is inclined upward, the lower outlet 6 is inclined downward, and the upper outlet 5 is located above the lower outlet 6. The upper outlet 5 is a cylindrical hole, and two upper outlets 5 are provided, and the two upper outlets 5 are symmetrical. The lower outlet 6 is a cylindrical hole, and two lower outlets 6 are provided, and the two lower outlets 6 are symmetrical.

[0036] The angle between the upper outlet 5 and the axis of the body is α, 50°≤α≤80°; the angle between the lower outlet 6 and the axis of the body is β, 55°≤β≤85°. The distance between the upper outlet 5 and the lower outlet 6 is S, 50mm≤α≤150mm.

[0037] The argon blowing system includes an inlet pipe 2, a down pipe 3 and an outlet pipe 4. The inlet pipe 2 is connected to the argon pipeline, the inlet pipe 2 extends horizontally into the upper part of the side wall of the body, the down pipe 3 is vertically arranged on the side wall of the body, the top of the down pipe 3 is connected to the inlet pipe 2, the bottom of the down pipe 3 is located at the upper outlet 5, and the bottom of the down pipe 3 is connected to the horizontal outlet pipe 4. Argon enters from the inlet pipe 2, passes through the down pipe 3, and is ejected from the outlet pipe 4.

[0038] The outlet of the immersion water inlet of the present invention is composed of an upper outlet 5 and a lower outlet 6. The outlet angle of the upper outlet 5 is upward, and the molten steel flowing out of it flows through the molten steel surface of the crystallizer 7 and then goes down into the deep liquid phase hole. The outlet angle of the lower outlet 6 is downward, and a small part of the molten steel flowing out of it flows to the billet shell, and most of it directly goes down into the deep liquid phase hole.

[0039] Argon enters from the argon blowing system inlet pipe 2, and is ejected from the outlet pipe 4 through the lower pipe 3, and is blown into the molten steel to form argon bubbles. Its function is to adjust the flow rate of the molten steel flowing out through the upper outlet 5. The larger the argon blowing amount, the smaller the molten steel flow rate, and vice versa. In this way, the flow rate of the molten steel flowing through the molten steel surface of the crystallizer can be adjusted, thereby adjusting the slag melting speed of the protective slag, reducing the liquid level fluctuation, and further controlling the quality of the ingot.

[0040] A method for improving the quality of a casting is implemented based on the above-mentioned submerged nozzle for improving the quality of a casting, and specifically comprises the following steps:

[0041] 1) Bake the immersion nozzle before use;

[0042] 2) Install the submerged nozzle on the tundish, and connect the argon blowing system air inlet pipe to the argon gas pipeline;

[0043] 3) Before pouring, turn on the argon blowing system. Argon enters from the air inlet pipe, passes through the lower pipe, and is ejected from the air outlet pipe;

[0044] 4) Start pouring and adjust the argon flow rate according to the slag melting and the crystallizer liquid level fluctuation during the continuous casting process. When the crystallizer liquid level fluctuation is greater than ±5mm, increase the argon flow rate by 10% to 90%; conversely, when the melting of the protective slag at the crystallizer liquid level is more than 10% lower than the set value, reduce the argon flow rate by 10% to 90% until the continuous casting ends.

[0045] When the flow rate of molten steel flowing out of the upper outlet 5 is too large, the fluctuation amplitude of the crystallizer liquid level will increase, and the melting rate of the protective slag will also be too large. When the fluctuation amplitude of the crystallizer liquid level is greater than the control range, the argon flow rate is increased to reduce the flow rate of molten steel flowing out of the upper outlet 5; conversely, when the protective slag on the crystallizer liquid surface melts too slowly, the argon flow rate is increased to increase the flow rate of molten steel flowing out of the upper outlet 5.

[0046] The advantages of the present invention are as follows: ① The flow rate of the stream flowing through the liquid surface can be adjusted at any time, which is beneficial to the quality control of the ingot; ② The amount of "head-on collision" of the molten steel flow near the immersed water nozzle will be greatly reduced, so the slag rolling phenomenon will be greatly reduced: the flow stream collision of the liquid surface near the water nozzle will be reduced or even eliminated; ③ The molten steel flow flowing out of the upper outlet 5 directly flows through the liquid surface and contacts with the protective slag, instead of first impacting the narrow edge of the ingot shell and then returning to the liquid surface as in the original method, so the structure of the present invention will reduce the chance of inclusions being captured by the solidification front of the ingot shell, thereby reducing the inclusion content of the ingot; ④ The molten steel flow flowing out of the upper outlet 5 directly flows through the liquid surface to reach the steel liquid surface of the crystallizer, and the liquid flow will become stable, so the fluctuation amplitude of the steel liquid surface of the crystallizer will be significantly reduced, reducing the occurrence of slag inclusion in the ingot shell, and at the same time reducing the depth of the vibration mark; ⑤ The impact of the stream on the ingot shell is reduced, the uneven thickness of the ingot shell is improved, and the occurrence of defects such as longitudinal cracks is reduced; ⑥ The liquid surface temperature is higher, which is beneficial to accelerate the melting of the protective slag.

[0047] Embodiment 1:

[0048] Continuous casting of automobile steel slabs, slab specifications, width: 1550mm, thickness: 300mm.

[0049] 1. Prepare an immersion nozzle, the upward angle of the upper outlet 5 is: the angle α with the axis of the immersion nozzle is 60°. The downward angle of the lower outlet 6 is: the angle β with the axis of the immersion nozzle is 65°. The distance S between the upper and lower outlets is 85mm.

[0050] 2. Bake the immersion nozzle before use.

[0051] 3. Install the submerged nozzle on the tundish, and connect the argon blowing system air inlet pipe 2 to the argon gas pipeline;

[0052] 4. Before pouring, turn on the argon blowing system. Argon gas enters from the air inlet pipe 2, passes through the down pipe 3, and flows out from the air outlet pipe 4.

[0053] 5. Start pouring. During the continuous casting process, adjust the argon flow rate to 3.0L / min according to the slag slagging condition and the meniscus liquid level fluctuation;

[0054] 6.Continue casting until the end.

[0055] After low-power inspection and purity inspection, the surface and internal quality of the ingot is significantly better than that of the ingot made by the traditional submerged nozzle. The total oxygen content is reduced from 0.0029% to 0.0018%, the large particle inclusions are reduced by 72%, the vibration mark depth is reduced by about 1.2mm, the slag inclusion defect rate is reduced by 65%, and the incidence of longitudinal crack defects is reduced from 0.02 times / casting to 0 times.

[0056] Embodiment 2:

[0057] Continuous casting of ship steel slabs, slab specifications, width: 1600mm, thickness: 230mm.

[0058] 1. Prepare an immersion nozzle. The upward angle of the upper outlet 5 is: the angle α with the axis of the immersion nozzle is 70°. The downward angle of the lower outlet 6 is: the angle β with the axis of the immersion nozzle is 60°. The distance S between the upper and lower outlets is 95mm;

[0059] 2. Bake the immersion nozzle before use;

[0060] 3. Install the submerged nozzle on the tundish, and connect the argon blowing system air inlet pipe 2 to the argon gas pipeline;

[0061] 4. Before pouring, turn on the argon blowing system. Argon enters from the air inlet pipe 2, passes through the down pipe 3, and flows out from the air outlet pipe 4;

[0062] 5. Start pouring. During the continuous casting process, adjust the argon flow rate to 4.5L / min according to the slag slagging condition and the meniscus liquid level fluctuation;

[0063] 6.Continue casting until the end.

[0064] After low-power inspection and purity inspection, the surface and internal quality of the ingot is significantly better than that of the ingot made by the traditional submerged nozzle. The total oxygen content is reduced from 0.0032% to 0.0020%, the large particle inclusions are reduced by 75%, the vibration mark depth is reduced by about 1.0mm, the slag inclusion defect rate is reduced by 77%, and the incidence of longitudinal crack defects is reduced from 0.015 times / casting to 0 times.

[0065] The present invention can eliminate the vortex generated by the liquid steel surface in the crystallizer during continuous steel casting, prevent the inclusion of protective slag, and at the same time, reduce the impact of the flow stream on the billet shell, improve the uneven thickness of the billet shell, and reduce the occurrence of defects such as longitudinal cracks. The present invention can significantly improve the quality of the billet.

[0066] The protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent substitutions or changes according to the technical solution and inventive concept of the present invention within the technical scope disclosed by the present invention, and all of them should be covered by the protection scope of the present invention.

Claims

1. An immersion nozzle for improving the quality of the casting, characterized in that: Including submerged nozzle and argon blowing system; The body of the immersion nozzle is a long tube with an open top and a closed bottom. The lower part of the body is provided with an upper outlet and a lower outlet; The upper outlet is inclined upward, the lower outlet is inclined downward, and the upper outlet is located above the lower outlet; The argon blowing system comprises an air inlet pipe, a down pipe and an air outlet pipe; The air inlet pipe is connected to the argon gas pipeline, the air inlet pipe extends into the upper part of the side wall of the main body, the down pipe is vertically arranged on the side wall of the main body, the top of the down pipe is connected to the air inlet pipe, the bottom of the down pipe is located at the upper outlet, and the bottom of the down pipe is connected to the air outlet pipe; Argon gas enters from the air inlet pipe, passes through the downpipe, and is ejected from the air outlet pipe.

2. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The angle between the upper outlet and the axis of the body is α, 50°≤α≤80°.

3. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The included angle between the lower outlet and the axis of the body is β, 55°≤β≤85°.

4. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The distance between the upper outlet and the lower outlet is S, 50mm≤α≤150mm.

5. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The upper outlet is composed of two holes which are symmetrical.

6. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The lower outlet is composed of two holes which are symmetrical.

7. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The submerged nozzle is installed on the tundish.

8. The submerged nozzle for improving the quality of the casting according to claim 1, characterized in that: The upper part of the body is trumpet-shaped, and the lower part is straight-cylindrical.

9. A method for improving the quality of a casting, which is realized based on the submerged nozzle for improving the quality of a casting according to any one of claims 1 to 8, characterized in that: The specific steps include: 1) Bake the immersion nozzle before use; 2) Install the submerged nozzle on the tundish, and connect the argon blowing system air inlet pipe to the argon gas pipeline; 3) Before pouring, turn on the argon blowing system. Argon enters from the air inlet pipe, passes through the lower pipe, and is ejected from the air outlet pipe; 4) During the pouring and continuous casting process, the argon flow rate is adjusted according to the slagging of the protective slag and the fluctuation of the liquid level in the crystallizer.

10. A method for improving the quality of a casting according to claim 9, characterized in that: In the step 4), when the fluctuation amplitude of the crystallizer liquid level is greater than ±5 mm, the argon flow rate is increased by 10% to 90%; conversely, when the melting of the protective slag at the crystallizer liquid level is more than 10% lower than the set value, the argon flow rate is reduced by 10% to 90% until the continuous casting is completed.

Citation Information

Patent Citations

  • Continuous casting production technology for producing wide and thick-cross section pipeline steel casting blank

    CN109014168A

  • Device for eliminating eddy slag entrapment of slab continuous casting crystallizer and using method

    CN118162609A

  • Continuous casting method

    JP1990121757A

  • Immersion nozzle for continuous casting and continuous casting method of steel

    JP2000237851A

  • Immersion nozzle for continuous casting and method for steel continuous casting

    JP2019063851A