Welding method for double-wire submerged-arc automatic welding double-face single-pass welding
The double-sided single-pass welding method of double-wire submerged arc automatic welding solves the problems of high equipment cost, poor flexibility and low welding efficiency of existing welding methods in steel plate splicing, and achieves no primer and no carbon planing. Efficient welding, adapts to the welding needs of steel plates of different thicknesses, and improves welding efficiency and melting efficiency.
Patent Information
- Application Number
- CN202411028125.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-01
AI Technical Summary
Existing welding methods such as FCB method, FAB method and single-wire submerged arc automatic welding have the problems of high equipment cost, poor flexibility, narrow material coverage and low welding efficiency in steel plate splicing, especially in the thickness and material diversity of steel plates. application challenges.
Double-wire submerged arc automatic welding double-sided single-pass welding method is adopted. Different groove types and power supply configurations are selected according to the thickness of the steel plate. Through cutting and assembly, welding without primer and carbon-free root planing is achieved, using DC and AC The power supply supplies power to welding wires of different diameters evenly, and adjusts the welding current, voltage and speed to match the welding parameters to ensure penetration of the weld without welding through.
It can reduce the angular deformation of the steel plate and improve the welding efficiency without the need for bottom welding and carbon planing. It can adapt to the welding needs of steel plates of different thicknesses and improve the melting efficiency and welding efficiency.
Smart Images

Figure CN118720352A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding, and relates to a double-wire submerged arc automatic welding double-sided single-pass welding method, in particular to a control implementation method for butt welding of steel plates with a thickness between 6mm and 28mm. Background Art
[0002] In the construction of ships, marine engineering, bridges and other engineering projects, large-width steel plates are often spliced. Commonly used welding methods include flux copper backing single-sided welding (FCB method: Flux Copper Backing), single-sided welding double-sided forming submerged arc welding (FAB method: Flux Asbest Backing), single-wire submerged arc automatic welding, etc. Each welding method has its own advantages and disadvantages.
[0003] FCB welding is an efficient method of panel assembly. It mainly covers steel plates with a thickness of 10mm to 40mm. It adopts a Y-shaped groove and is welded in one step. Its advantages are high welding efficiency and good welding quality. It is often used for butt welding of large steel plates. However, the construction cost of the FCB production line is very high, the equipment is very expensive, the site is fixed, it cannot be moved, and the flexibility is poor.
[0004] FAB welding uses V-shaped grooves, with high welding efficiency, common equipment, and flexible promotion and use. However, the thickness of steel plates that can be welded by FAB welding is usually 9mm to 30mm, and the material can only cover A, AH32 and AH36, so the application range is relatively narrow.
[0005] Single-wire submerged arc automatic welding can select the appropriate groove form according to the thickness of the steel plate, and use single or multiple passes to splice the steel plate. It is also the main welding method for splicing plates, and the thickness of the steel plate varies from a few millimeters to hundreds of millimeters. However, the welding efficiency is lower than that of the FCB method and the FAB method.
[0006] In actual use, the FCB method requires too high an investment in equipment and infrastructure, and has a long construction period; the FAB method is more flexible, but the materials it can cover are limited; single-wire submerged arc automatic welding has a wide range of uses, but compared to the FCB and FAB methods, its welding efficiency is relatively low. Summary of the invention
[0007] The purpose of the present invention is to provide a double-wire submerged arc automatic welding double-sided single-pass welding method, which effectively solves the problems existing in the FCB method, the FAB method and the single-wire submerged arc automatic welding.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0009] The invention discloses a double-wire submerged arc automatic double-sided single-pass welding method, which selects different groove types according to the different thicknesses of steel plates, cuts, assembles and welds them.
[0010] When welding and splicing steel plates with a thickness of 6mm-12mm, a stable single submerged arc power supply with a maximum output current of 1000A-1500A is used. Two submerged arc welding wires with a diameter of 1.6mm are evenly powered at the same time to form a double-wire single molten pool. The I-shaped groove is welded. No welding primer is performed when welding on the front side, and no carbon planing is performed when turning over for back welding.
[0011] When welding and splicing steel plates with a thickness of 10mm-20mm, two stable submerged arc power supplies with a maximum output current of 1000A-1500A are used to power two submerged arc welding wires with a diameter of 4.0mm respectively, forming a double-wire single molten pool, and welding is performed on the I-shaped grooves that are cut and assembled. No welding primer is performed when welding on the front side, and no carbon planing is performed when turning over for back side welding.
[0012] When welding and splicing steel plates with a thickness of 20mm-28mm, two stable submerged arc power supplies with a maximum output current of 1000A-1500A are used to power two submerged arc welding wires with a diameter of 4.0mm respectively, forming a double-wire single molten pool, and welding is performed on the Y-shaped grooves that are cut and assembled. No welding primer is performed when welding on the front side, and no carbon planing is performed when turning over for back welding.
[0013] Furthermore, when the thickness of the steel plate is 6mm-20mm, the gap of the assembled I-type groove is controlled at 0mm-1mm, and the natural groove angle is controlled at 0°-6°; when the thickness of the steel plate is 20mm-26mm, the gap of the assembled Y-type groove is controlled at 0mm-1mm, the groove angle is controlled at 55°-65°, and the blunt edge height is controlled at 15mm-17mm; when the thickness of the steel plate is 26mm-28mm, the gap of the assembled Y-type groove is controlled at 0mm-1mm, the groove angle is controlled at 55°-65°, and the blunt edge height is controlled at 17mm-19mm.
[0014] Furthermore, when welding steel plates with a thickness of 6mm-12mm, the submerged arc power supply used is a DC power supply; when welding steel plates with a thickness of 10mm-28mm, the first submerged arc power supply that powers the first submerged arc welding wire is a DC power supply, and the second submerged arc power supply that powers the second submerged arc welding wire is an AC power supply.
[0015] Furthermore, when a single submerged arc power source and a double submerged arc welding wire with a diameter of 1.6 mm are used to perform double-sided single-pass welding of steel plates with a thickness of 6 mm-12 mm assembled into an I-shaped groove, appropriate welding current, welding voltage and welding speed are selected to match each other to ensure that the weld is welded through without welding primer and carbon planing root cleaning. The matching welding parameters are shown in Table 1. For steel plates of other thicknesses, the nearest parameters can be selected for matching and appropriate adjustments can be made.
[0016] Table 1 Welding parameters of steel plates with different thicknesses.
[0017]
[0018] Furthermore, when a double submerged arc power source and a double submerged arc welding wire with a diameter of 4.0 mm are used to perform double-sided single-pass welding of steel plates with a thickness of 10 mm-20 mm assembled into an I-shaped groove, appropriate welding current, welding voltage and welding speed are selected to match each other to ensure that the weld is welded through without welding primer and carbon planing root cleaning. The matching welding parameters are shown in Table 2. For other thickness steel plates, the nearest parameters are selected for matching and appropriate adjustments can be made.
[0019] Table 2 Welding parameters of steel plates with different thicknesses.
[0020]
[0021] Furthermore, when a double submerged arc power source and a double submerged arc welding wire with a diameter of 4.0 mm are used to perform double-sided single-pass welding of steel plates with a thickness of 20 mm-26 mm assembled into a Y-shaped groove, appropriate welding current, welding voltage and welding speed are selected to match each other to ensure that the weld is welded through without welding primer and carbon planing root cleaning. The matching welding parameters are shown in Table 3. For other thickness steel plates, the nearest parameters can be matched and adjusted appropriately.
[0022] Table 3 Welding parameters of steel plates with different thicknesses.
[0023]
[0024] Furthermore, when a double submerged arc power source and a double submerged arc welding wire with a diameter of 4.0 mm are used to perform double-sided single-pass welding of steel plates with a thickness of 26 mm-28 mm assembled into a Y-shaped groove, appropriate welding current, welding voltage and welding speed are selected to match each other to ensure that the weld is welded through without welding primer and carbon planing root cleaning. The matching welding parameters are shown in Table 4. For other thickness steel plates, the nearest parameters can be selected for matching and appropriate adjustments can be made.
[0025] Table 4 Welding parameters of steel plates with different thicknesses.
[0026]
[0027] Furthermore, for a conductive tip using two submerged arc welding wires with a diameter of 1.6 mm, the length of the welding wire rod is 20 mm-30 mm, and the welding wire spacing is 6 mm-8 mm.
[0028] Further, for a conductive structure using two submerged arc welding wires with a diameter of 4.0 mm, the forward tilt angle of the first submerged arc welding wire is 8°-9°, and the length of the welding wire rod is 30 mm-40 mm; the backward tilt angle of the second submerged arc welding wire is 13°-16°, and the length of the welding wire rod is 35 mm-45 mm. The spacing between the two submerged arc welding wires with a diameter of 4.0 mm is 28 mm-32 mm.
[0029] Furthermore, the fusion cross length of the front welding and the back welding under the welding conditions of the benchmark welding parameters obtained in the experiment is controlled within a range of 4mm-6mm to ensure that the fusion overlap of the front welding and the back welding can still be guaranteed when the welding parameters fluctuate and the assembly status differs, thereby achieving the goal of welding through without carbon planing.
[0030] Compared with the prior art, the beneficial technical effects of the present invention are:
[0031] (1) The present invention realizes double-sided single-pass welding by controlling the assembly gap and reasonably adjusting the matching of welding current, welding voltage and welding speed. It does not require base welding or carbon planing to clean the root, and double-sided single-pass welding is formed in one step. This reduces the angular deformation of the spliced steel plates and the workload of deformation adjustment.
[0032] (2) Based on single-wire submerged arc automatic welding, the present invention improves melting efficiency and welding efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the I-type groove structure of the present invention.
[0034] Figure 2 It is a schematic diagram of the Y-shaped groove structure of the present invention.
[0035] Figure 3 The figure is a schematic diagram of the corrosion of the weld section after the groove welding of the present invention is completed. In the figure, 1 refers to the first front welding, and 2 refers to the second back welding.
[0036] Figure 4 It is a schematic diagram of a single power source dual submerged arc welding wire conductive nozzle of the present invention.
[0037] Figure 5 It is a schematic diagram of the conductive structure of the dual power source dual submerged arc welding wire of the present invention. DETAILED DESCRIPTION
[0038] In order to facilitate understanding of the technical solution of the present invention, some technical terms in the present invention are first explained: (1) Natural bevel: refers to a bevel that is not desired to exist. It is best not to have such a bevel, but it is difficult to avoid in the actual production process or avoiding such a bevel will incur a very high cost, so a certain degree of bevel can be accepted. (2) Bevel: refers to a bevel that is expected to be opened, which is actually needed. (3) Benchmark: refers to the ideal value during design, but in actual production, a certain degree of deviation is allowed based on the benchmark value, for example: if the benchmark angle is 60°, the angle during actual production can be 60±3°; if the benchmark height is 16mm, the height during actual production can be 16±1mm.
[0039] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0040] Embodiment 1: A double-wire submerged arc automatic double-sided single-pass welding method, according to the different thickness of the steel plate, select different groove types, cut and complete assembly and welding.
[0041] When the steel plate thickness is 6mm-12mm, the cutting assembly is an I-type groove, such as Figure 1 As shown, the gap G is controlled at 0mm-1mm, and the natural groove angle α is controlled at 0°-6°. Two submerged arc welding wires with a diameter of 1.6mm are selected, and a stable single DC power supply with a maximum output current of 1250A is used to evenly power the two submerged arc welding wires at the same time. Figure 4 As shown, the wire rod length h5 is 25 mm and the wire spacing L1 is 7 mm.
[0042] When the steel plate thickness is 10mm-20mm, cut and assemble into I-type groove, such as Figure 1 As shown, the gap G is controlled within 0mm-1mm, and the natural groove angle α is controlled within 6°. Two submerged arc welding wires with a diameter of 4.0mm are selected, and the two submerged arc welding wires are the first submerged arc welding wire and the second submerged arc welding wire. A DC power supply with a maximum output current of 1500A is used to power the first submerged arc welding wire, and an AC power supply with a maximum output current of 1250A is used to power the second submerged arc welding wire. Figure 5 As shown, the forward tilt angle α1 of the first submerged arc welding wire is 8°, and the wire rod length h6 is 35 mm; the backward tilt angle α2 of the second submerged arc welding wire is 15°, and the wire rod length h7 is 40 mm. The distance L2 between the two submerged arc welding wires with a diameter of 4.0 mm is 30 mm.
[0043] Since the equipment used for welding with a submerged arc welding wire with a diameter of 4.0 mm is the same, the configuration angle of the submerged arc welding wire is also the same, only the groove form and parameters are changed, so the fixing form of the submerged arc welding wire for the I-type groove with a steel plate thickness of 10 mm-20 mm is the same as the fixing form of the submerged arc welding wire for the Y-type groove with a steel plate thickness of 20 mm-28 mm. Figure 5 shown.
[0044] When the steel plate thickness is 20mm-26mm, cut and assemble into a Y-shaped groove, such as Figure 2 As shown, the gap G is controlled at 0mm-1mm, the groove angle β is 60°, and the blunt edge height h is 16mm. Two submerged arc welding wires with a diameter of 4.0mm are selected, and the two submerged arc welding wires are the first submerged arc welding wire and the second submerged arc welding wire. A DC power supply with a maximum output current of 1500A is used to power the first submerged arc welding wire, and an AC power supply with a maximum output current of 1250A is used to power the second submerged arc welding wire. Figure 5 As shown, the forward tilt angle α1 of the first submerged arc welding wire is 8°, and the wire rod length h6 is 35 mm; the backward tilt angle α2 of the second submerged arc welding wire is 15°, and the wire rod length h7 is 40 mm. The distance L2 between the two submerged arc welding wires with a diameter of 4.0 mm is 30 mm.
[0045] When the steel plate thickness is 26mm-28mm, cut and assemble into a Y-shaped groove, such as Figure 2 As shown, the gap G is controlled at 0mm-1mm, the groove angle β is 60°, and the blunt edge height h is 18mm. Two submerged arc welding wires with a diameter of 4.0mm are selected, and the two submerged arc welding wires are the first submerged arc welding wire and the second submerged arc welding wire. A DC power supply with a maximum output current of 1500A is used to power the first submerged arc welding wire, and an AC power supply with a maximum output current of 1250A is used to power the second submerged arc welding wire. Figure 5 As shown, the forward tilt angle α1 of the first submerged arc welding wire is 8°, and the wire rod length h6 is 35 mm; the backward tilt angle α2 of the second submerged arc welding wire is 15°, and the wire rod length h7 is 40 mm. The distance L2 between the two submerged arc welding wires with a diameter of 4.0 mm is 30 mm.
[0046] Based on the above preparation conditions, the test process is explained by taking the steel plate with a thickness of 16 mm as an example.
[0047] Cut and assemble the 16mm steel plate into an I-shaped groove, such as Figure 1As shown, the gap is controlled within 1mm, the natural angle α is controlled within 6°, and two submerged arc welding wires with a diameter of 4.0mm are selected. The two submerged arc welding wires are the first submerged arc welding wire and the second submerged arc welding wire. A DC power supply with a maximum output current of 1500A is used to power the first submerged arc welding wire, and an AC power supply with a maximum output current of 1250A is used to power the second submerged arc welding wire. Figure 5 As shown, the forward tilt angle α1 of the first submerged arc welding wire is 8°, and the wire rod length h6 is 35 mm; the backward tilt angle α2 of the second submerged arc welding wire is 15°, and the wire rod length h7 is 40 mm. The distance L2 between the two submerged arc welding wires with a diameter of 4.0 mm is 30 mm.
[0048] Welding of the assembled 16mm thick steel plate was started. During the welding process, the welding current, welding voltage and welding speed of the first and second submerged arc welding wires were constantly adjusted, and records were made in sections. After the front welding was completed, the steel plate was cut in sections, and the cross section of the steel plate was polished and corroded. Figure 3 As shown, the weld excess height h1 is selected to be less than 3 mm, the weld appearance is uniform, and the fusion depth h4 is greater than half of the steel plate thickness, that is, the welding parameters of this section are selected as the benchmark welding parameters for front welding.
[0049] After selecting the reference welding parameters for front welding, re-weld a pair of 16mm thick steel plates according to these welding parameters, and then weld the back side. Also, during the welding process, the welding current, welding voltage and welding speed of the first submerged arc welding wire and the second submerged arc welding wire are constantly adjusted, and records are made in sections. After welding, the steel plate is cut in sections, and the cross section of the steel plate is polished and corroded. Figure 3 As shown, the welding parameters in the area where the excess height h2 is less than 3 mm, the weld appearance is uniform, and the fusion cross length h3 of the front welding and the back welding is between 4 mm and 5 mm are selected as the reference welding parameters for the back welding.
[0050] Finally, the benchmark welding parameters for the 16 mm thick steel plate are determined as shown in Table 5.
[0051] Table 5 Benchmark welding parameters for 16 mm thick steel plate.
[0052]
[0053] The reference welding parameters (such as Table 5) are approximate intermediate values of the welding parameters (such as Table 2) corresponding to the plate thickness. It is necessary to first obtain the reference welding parameters through experimental exploration, and then expand the parameter range based on the reference welding parameters according to the specification requirements, so that the effect achieved is: within the range of welding parameters, any welding current, welding voltage, and welding speed can be used for combined welding to obtain an acceptable weld appearance and a weld penetration effect.
[0054] In fact, what determines the weld penetration is the welding heat input, that is, the heat energy obtained on the unit length of the weld, E = (60U1I1+60U2I2) / (1000V), where the unit of heat input E is KJ / mm, the unit of voltage U is volt (V), the unit of current I is ampere (A), and the unit of welding speed V is mm / min.
[0055] Taking a 16mm thick steel plate as an example, after obtaining the benchmark welding parameters (Table 5) in the test, the heat input of 3.9943KJ / mm for the 16mm steel plate during front welding will be calculated. According to the classification society's requirements, when the heat input does not exceed 5KJ / mm, the heat input can fluctuate within the range of ±25%; when the heat input exceeds 5KJ / mm, the heat input can fluctuate within the range of -25% to +10%. Therefore, the calculated heat input range is 2.9957KJ / mm to 4.9929KJ / mm. According to common experience, when the double-wire submerged arc automatic welding is less than 20mm, the upper and lower floating range of the welding current is generally controlled at about ±10%, rounded and the single digit is adjusted to 0 and 5; the upper and lower floating range of the welding voltage is generally controlled at about ±7%, and the last digit is adjusted to 0 or 0.5; when the double-wire submerged arc automatic welding is 20mm and above, the upper and lower floating range of the welding current is generally controlled at about ±5%, rounded and the single digit is adjusted to 0 and 5; the upper and lower floating range of the welding voltage is generally controlled at about ±3.5%, and the last digit is adjusted to 0 or 0.5. Therefore, the welding current ranges of the first and second electrodes (i.e., the first and second submerged arc power sources) on the front are calculated to be 630A~770A and 450A~550A respectively; the welding voltages of the first and second electrodes on the front are calculated to be 35.5V~40.5V and 37V~43V respectively. Then, based on the above heat input range, welding current range, and welding voltage range, the welding speed range is calculated to be 661 mm / min to 780 mm / min. Similarly, the heat input on the back of the steel plate is 4.5429KJ / mm, and it floats according to the heat input ±25%. The welding heat input range is 3.4071KJ / mm~5.6786KJ / mm. The heat input exceeds 5KJ / mm, so the upward floating needs to float according to +10%, that is, the welding heat input range is 3.4071KJ / mm~4.9971KJ / mm. According to common experience, for double-wire submerged arc automatic welding below 20mm, the upper and lower floating range of welding current is generally controlled at about ±10%, rounded and the single digit is adjusted to 0 and 5; the upper and lower floating range of welding voltage is generally controlled at about ±7%, and the last digit is adjusted to 0 or 0.5. For double-wire submerged arc automatic welding of 20mm and above, the upper and lower floating range of welding current is generally controlled at about ±5%, rounded and the single digit is adjusted to 0 and 5; the upper and lower floating range of welding voltage is generally controlled at about ±3.5%, and the last digit is adjusted to 0 or 0.5. Therefore, the welding current ranges of the first and second electrodes on the back are calculated to be 720A~880A and 450A~550A respectively; the welding voltages of the first and second electrodes on the back are calculated to be 37V~43V and 39V~45V respectively. Then, based on the above heat input range, welding current range, and welding voltage range, the welding speed range is calculated to be 663mm / min~777mm / min.In summary, based on the data in Table 5 obtained from the test, the welding parameter range corresponding to the 16 mm thick steel plate in Table 2 was calculated.
[0056] Similarly, the benchmark welding parameters of steel plates of various other thicknesses were measured experimentally, and the corresponding heat input was calculated using the calculation formula E=(60U1I1+60U2I2) / (1000V), where the unit of heat input E is KJ / mm, the unit of voltage U is volt (V), the unit of current I is ampere (A), and the unit of welding speed V is mm / min. The allowable range of heat input was calculated according to the requirements of classification society regulations, that is, when the heat input does not exceed 5KJ / mm, the heat input can float within the range of ±25%, and when the heat input exceeds 5KJ / mm, the heat input can float within the range of -25% to +10%.
[0057] According to common experience, when welding twin-wire submerged arc welding with a diameter of less than 20 mm, the upper and lower floating range of welding current is generally controlled at around ±10%, rounded up and the unit digit adjusted to 0 and 5 as nearest; the upper and lower floating range of welding voltage is generally controlled at around ±7%, and the last digit is adjusted to 0 or 0.5 as nearest; when welding twin-wire submerged arc welding with a diameter of 20 mm or more, the upper and lower floating range of welding current is generally controlled at around ±5%, rounded up and the unit digit adjusted to 0 and 5 as nearest; the upper and lower floating range of welding voltage is generally controlled at around ±3.5%, and the last digit is adjusted to 0 or 0.5 as nearest, to determine the floating range of welding current and welding voltage.
[0058] Finally, based on the heat input range, welding current range, and welding voltage range obtained by the above calculation, the range of welding speed is reversely calculated according to the above calculation formula, wherein the minimum value of heat input, the minimum value of welding current, and the minimum value of welding voltage are taken to calculate the maximum value of welding speed; the maximum value of heat input, the maximum value of welding current, and the maximum value of welding voltage are taken to calculate the minimum value of welding speed.
[0059] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A double-wire submerged arc automatic welding double-sided single-pass welding method, characterized in that: According to the thickness of steel plates, different groove types are selected, cut, assembled and welded; When the thickness of the steel plate is 6mm-12mm, a stable single submerged arc power supply with a maximum output current of 1000A-1500A is used to power two submerged arc welding wires with a diameter of 1.6mm at the same time to form a double-wire single molten pool, and the groove assembled into I type is welded without welding primer and carbon planer root cleaning; When the thickness of the steel plate is 10mm-20mm, two stable submerged arc power supplies with a maximum output current of 1000A-1500A are used to power two submerged arc welding wires with a diameter of 4.0mm, forming a double-wire single molten pool, and welding the I-shaped grooves without welding primer and carbon planing root cleaning; When the steel plate thickness is 20mm-28mm, two stable submerged arc power supplies with a maximum output current of 1000A-1500A are used to power two submerged arc welding wires with a diameter of 4.0mm respectively, forming a double-wire single molten pool, and welding the Y-shaped grooves assembled by cutting, without the need for welding primer and carbon planer root cleaning.
2. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 1, characterized in that: When the thickness of the steel plate is 6mm-20mm, the gap of the assembled I-type groove is controlled at 0mm-1mm, and the natural groove angle is controlled at 0°-6°; When the thickness of the steel plate is 20mm-26mm, the gap of the Y-shaped groove is controlled at 0mm-1mm, the groove angle is controlled at 55°-65°, and the blunt edge height is controlled at 15mm-17mm; When the thickness of the steel plate is 26mm-28mm, the gap of the assembled Y-shaped groove is controlled at 0mm-1mm, the groove angle is controlled at 55°-65°, and the blunt edge height is controlled at 17mm-19mm.
3. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 2 is characterized in that: When welding steel plates with a thickness of 6mm-12mm, the submerged arc power source used is a DC power source; When welding steel plates with a thickness of 10mm-28mm, the first submerged arc power supply for supplying power to the first submerged arc welding wire is a DC power supply, and the second submerged arc power supply for supplying power to the second submerged arc welding wire is an AC power supply.
4. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 3 is characterized in that: When a single submerged arc power source and a double submerged arc welding wire with a diameter of 1.6 mm are used to weld a steel plate with a thickness of 6 mm to 12 mm and assembled into an I-shaped groove, the welding parameters including welding current, welding voltage and welding speed are set as follows: When the thickness of the steel plate is 6mm, the welding current of the front welding is 450-550A, the welding voltage is 30.5-35.5V, and the welding speed is 1037-1193mm / min. The welding current of the back welding is 540-660A, the welding voltage is 31.5-36.5V, and the welding speed is 951-1109mm / min. When the thickness of the steel plate is 8mm, the welding current of the front welding is 495-605A, the welding voltage is 31.5-36.5V, and the welding speed is 855-1005mm / min. The welding current of the back welding is 585-715A, the welding voltage is 32.5-37.5V, and the welding speed is 856-1000mm / min. When the thickness of the steel plate is 10mm, the welding current of the front welding is 540-660A, the welding voltage is 32.5-37.5V, and the welding speed is 946-1108mm / min. The welding current of the back welding is 630-770A, the welding voltage is 33.5-38.5V, and the welding speed is 847-1005mm / min. When the thickness of the steel plate is 12mm, the welding current of the front welding is 585-715A, the welding voltage is 33.5-38.5V, and the welding speed is 798-940mm / min. The welding current of the back welding is 675-825A, the welding voltage is 34.5-39.5V, and the welding speed is 706-836mm / min.
5. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 3 is characterized in that: When using a double submerged arc power source and a double submerged arc welding wire with a diameter of 4.0 mm to weld a steel plate with a thickness of 10 mm to 20 mm assembled into an I-shaped groove, the welding parameters including welding current, welding voltage and welding speed are set as follows: When the thickness of the steel plate is 10mm, the welding current of the first submerged arc power supply for front welding is 540-660A, the welding voltage is 31.5-36.5V, and the welding speed is 709-836mm / min. The welding current of the second submerged arc power supply for front welding is 425-515A, the welding voltage is 33.5-38.5V, and the welding speed is 709-836mm / min. The welding current of the first submerged arc power supply for back welding is 630-770A, the welding voltage is 31.5-36.5V, and the welding speed is 708-835mm / min. The welding current of the second submerged arc power supply for back welding is 405-495A, the welding voltage is 33.5-38.5V, and the welding speed is 708-835mm / min. When the thickness of the steel plate is 14 mm, the welding current of the first submerged arc power supply for front welding is 610-750A, the welding voltage is 32.5-37.5V, and the welding speed is 661-782mm / min. The welding current of the second submerged arc power supply for front welding is 415-505A, the welding voltage is 35.5-40.5V, and the welding speed is 661-782mm / min. The welding current of the first submerged arc power supply for back welding is 720-880A, the welding voltage is 35.5-40.5V, and the welding speed is 659-783mm / min. The welding current of the second submerged arc power supply for back welding is 450-550A, the welding voltage is 39-45V, and the welding speed is 659-783mm / min. When the thickness of the steel plate is 18 mm, the welding current of the first submerged arc power supply for front welding is 695-845 A, the welding voltage is 35.5-40.5 V, and the welding speed is 659-784 mm / min. The welding current of the second submerged arc power supply for front welding is 460-560 A, the welding voltage is 37-43 V, and the welding speed is 659-784 mm / min. The welding current of the first submerged arc power supply for back welding is 810-990 A, the welding voltage is 37-43 V, and the welding speed is 664-775 mm / min. The welding current of the second submerged arc power supply for back welding is 475-585 A, the welding voltage is 39-45 V, and the welding speed is 664-775 mm / min. When the thickness of the steel plate is 20mm, the welding current of the first submerged arc power supply for front welding is 810-880A, the welding voltage is 36.5-39.5V, and the welding speed is 687-854mm / min. The welding current of the second submerged arc power supply for front welding is 530-580A, the welding voltage is 38.5-41.5V, and the welding speed is 687-854mm / min. The welding current of the first submerged arc power supply for back welding is 905-975A, the welding voltage is 38.5-41.5V, and the welding speed is 677-853mm / min. The welding current of the second submerged arc power supply for back welding is 530-570A, the welding voltage is 40.5-43.5V, and the welding speed is 677-853mm / min.
6. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 3, characterized in that: When using a double submerged arc power source and a double submerged arc welding wire with a diameter of 4.0 mm to weld a steel plate with a thickness of 20 mm to 26 mm assembled into a Y-shaped groove, the welding parameters including welding current, welding voltage and welding speed are set as follows: When the thickness of the steel plate is 22 mm, the welding current of the first submerged arc power supply for front welding is 720-780 A, the welding voltage is 34.5-37.5 V, and the welding speed is 631-789 mm / min. The welding current of the second submerged arc power supply for front welding is 770-830 A, the welding voltage is 37.5-40.5 V, and the welding speed is 631-789 mm / min. The welding current of the first submerged arc power supply for back welding is 810-870 A, the welding voltage is 36.5-39.5 V, and the welding speed is 633-793 mm / min. The welding current of the second submerged arc power supply for back welding is 530-580 A, the welding voltage is 38.5-41.5 V, and the welding speed is 633-793 mm / min. When the thickness of the steel plate is 26mm, the welding current of the first submerged arc power supply for front welding is 770-830A, the welding voltage is 36.5-39.5V, and the welding speed is 584-730mm / min. The welding current of the second submerged arc power supply for front welding is 855-930A, the welding voltage is 38.5-41.5V, and the welding speed is 584-730mm / min. The welding current of the first submerged arc power supply for back welding is 905-985A, the welding voltage is 37.5-40.5V, and the welding speed is 583-732mm / min. The welding current of the second submerged arc power supply for back welding is 540-580A, the welding voltage is 39.5-42.5V, and the welding speed is 583-732mm / min.
7. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 3 is characterized in that: When using a double submerged arc power source and a double submerged arc welding wire with a diameter of 4.0 mm to weld a steel plate with a thickness of 26 mm to 28 mm assembled into a Y-shaped groove, the welding parameters including welding current, welding voltage and welding speed are set as follows: When the thickness of the steel plate is 28mm, the welding current of the first submerged arc power supply for front welding is 810-880A, the welding voltage is 36.5-39.5V, and the welding speed is 584-730mm / min. The welding current of the second submerged arc power supply for front welding is 855-925A, the welding voltage is 38.5-41.5V, and the welding speed is 584-730mm / min. The welding current of the first submerged arc power supply for back welding is 905-975A, the welding voltage is 38.5-41.5V, and the welding speed is 582-733mm / min. The welding current of the second submerged arc power supply for back welding is 570-620A, the welding voltage is 40.5-43.5V, and the welding speed is 582-733mm / min.
8. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 3, characterized in that: For a conductive tip using two submerged arc welding wires with a diameter of 1.6 mm, the wire rod length is 20 mm-30 mm, and the wire spacing is 6 mm-8 mm.
9. The double-wire submerged arc automatic double-sided single-pass welding method according to claim 3, characterized in that: For a conductive structure using two submerged arc welding wires with a diameter of 4.0 mm, the forward tilt angle of the first submerged arc welding wire is 8°-9°, and the length of the welding wire rod is 30 mm-40 mm; the backward tilt angle of the second submerged arc welding wire is 13°-16°, and the length of the welding wire rod is 35 mm-45 mm; The distance between two submerged arc welding wires with a diameter of 4.0 mm is 28 mm-32 mm.
Citation Information
Cited By
Machining method of medium-thickness plate austenitic stainless steel end socket
CN120395354A