Orthogonal laminated energetic film and 3D printing forming method

Using 3D printing technology to print energetic inks on plastic films in an orthogonal stacking manner solves the problem of structural unevenness of energetic films, achieves efficient combustion performance and molding quality, and ensures integrated design of materials and structures.

CN118721722APending Publication Date: 2024-10-01NANJING UNIV OF SCI & TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410778900.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When preparing energetic films, it is difficult to obtain a uniform and consistent structure, which affects its burning rate and energy release performance. Moreover, the process of controlling chemical composition, phase structure, and microstructure is complex and prone to deviations.

Method used

Using 3D printing technology, energetic inks are printed on plastic films in an orthogonal stacking manner, using N,N-dimethylformamide DMF as the solvent, polyylidene fluoride PVDF and thermoplastic polyurethane TPU as the dispersant. Nano-thermite and nano-titanium powder are mixed ultrasonically and solidified on a heating platform, and the printing parameters and microstructure are adjusted to optimize combustion performance.

Benefits of technology

It achieves reliable ignition, good molding structure and flexible shape fit of energetic films, promotes combustion performance, ensures integrated design of materials and structures, and improves combustion performance and molding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721722A_ABST
    Figure CN118721722A_ABST
Patent Text Reader

Abstract

The invention relates to an orthogonal laminated energetic film and a 3D printing forming method. The method comprises the following steps: (1) taking N, N-dimethylformamide (DMF) as a solvent, taking polyvinylidene fluoride (PVDF) and thermoplastic polyurethane (TPU) as dispersing agents, and performing ultrasonic mixing and uniform stirring on the N, N-DMF, PVDF and TPU to obtain a mixed solution; (2) adding a nano thermite and nano titanium powder into the mixed solution, and performing ultrasonic mixing and stirring to obtain energetic ink; and (3) the energetic ink is put into a needle cylinder, the plastic film is adsorbed to a heating platform through a vacuum pump, the 3D printing device is started, the energetic ink is printed on the plastic film in an orthographic lamination mode, and the energetic ink is cured at the temperature of 45-55 DEG C to form the energetic film. The method is simple and efficient, the orthographic laminated energetic film has the advantages of being good in performance, low in delay, high in energy release rate and the like, the design structures of the thermite and other energetic materials can be expanded, and the energetic film can better meet various application requirements of solid engines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid motors, and in particular relates to an orthogonal laminated energetic film and a 3D printing method. Background Art

[0002] Energetic film is a new structural form of energetic material, which is made of two or more different component materials that can undergo exothermic reactions and can undergo self-propagating exothermic reactions under external energy stimulation. Energetic film is mainly used as the primary electrothermal energy conversion element of ignition and detonation devices; as a local high-temperature heat source, energetic film can be used in the fields of microelectronic device welding, MEMS packaging, thermal batteries, and complex electronic device microstructure molding. The structural control of energetic film is crucial to its performance, but in the actual preparation process, it may be very difficult to obtain a uniform and consistent structure. This may affect the key performance indicators of the film, such as the burning rate and energy release. When preparing energetic films, it is necessary to precisely control the chemical composition, phase structure, and microstructure, all of which will affect the final performance of the film. However, these control processes can be very complex and prone to deviations.

[0003] The maturity of 3D printing technology, especially the direct ink writing (DIW) method, has allowed various material systems, such as functional materials, ceramics, metals, composites, biomaterials, energy materials and hydrogels, to be printed in specific 3D architectures. In general, the static properties of materials, such as stiffness and strength, or optical response, can be adjusted by designing and printing microstructures using 3D printing technology. The thermite reaction has been widely used as a representative gas-generating hot metal system under various synthetic techniques, experimental conditions and applications. When this reaction is energetically favorable, a large amount of excess energy is released in the form of heat and pressure, driving and accelerating the self-sustaining reaction. Summary of the invention

[0004] The object of the present invention is to provide an orthogonal laminated energetic film and a 3D printing method.

[0005] The technical solution to achieve the purpose of the present invention is: a 3D printing method for orthogonally stacked energetic films, comprising the following steps:

[0006] Step (1): using N,N-dimethylformamide (DMF) as a solvent, polyvinylidene fluoride (PVDF) and thermoplastic polyurethane (TPU) as dispersants, ultrasonically mixing the three, stirring them evenly, and obtaining a mixed solution;

[0007] Step (2): adding nano-thermite and nano-titanium powder to the mixed solution of step (1), and then performing ultrasonic mixing and stirring to obtain energetic ink;

[0008] Step (3): Place the energetic ink prepared in step (2) into a 2-10 ml syringe, use a vacuum pump to adsorb the plastic film onto the heating platform, start the 3D printing device, print the energetic ink on the plastic film in an orthogonal stacking manner, and cure the energetic ink at 45-55° C. for 60-120 min to form an energetic film.

[0009] Furthermore, in step (1), the mass of poly(vinylidene fluoride) PVDF is 0.8-1.0 g, the mass of thermoplastic polyurethane TPU is 0-0.2 g, and the mass of the solvent is 10-15 g.

[0010] Furthermore, the specific parameters of the ultrasonic mixing and stirring in step (1) are: ultrasonic mixing for 30-60 min, stirring for 30-60 min.

[0011] Furthermore, the mass ratio of the nano-thermite and the nano-titanium powder added in step (2) is 9:1, the nano-thermite includes nano-aluminum powder and nano-copper oxide powder, the mass ratio of the nano-aluminum powder and the nano-copper oxide powder is 1:3, and the added amount of the nano-aluminum powder is 1.9-2.1g.

[0012] Furthermore, the stirring in step (2) is carried out for 12±2 h.

[0013] Furthermore, the 3D printing device used in step (3) includes a three-dimensional motion platform and an MC600 motion controller.

[0014] Furthermore, in step (3), the ink is injected into the plastic film at an ink pushing speed of 0.77 μL / s-3.85 μL / s, and the needle movement speed is 5 mm / s-20 mm / s.

[0015] Furthermore, the orthogonal stacking method in step (3) is specifically as follows: under the condition of controlling the spacing, the printing directions of adjacent layers are perpendicular to each other.

[0016] An orthogonal stacked energetic film is prepared by the above method.

[0017] Compared with the prior art, the present invention has the following significant advantages:

[0018] (1) The present invention uses PVDF and TPU as dispersants, which can enhance the ability of the energetic ink to resist easy detachment from the plastic film after thermal curing, and can be bent arbitrarily to fit various shapes of propellant systems, thereby ensuring reliable ignition.

[0019] (2) The printing parameters and platform heating set in the present invention can ensure that the energetic ink is uniformly extruded when the needle moves, and can be quickly solidified when extruded onto the plastic film, so that the energetic ink has a good molding structure on the plastic film.

[0020] (3) The present invention adopts an orthogonal stacking method, which can adjust the printing design and microstructure, promote the gas flow during the combustion of the energetic film, thereby promoting the combustion performance of the energetic film, and can realize the integrated design of materials and structures according to needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the structure of the orthogonal stacked energetic film of the present invention; (a) is the main view, (b) is the side view, and (c) is the top view.

[0022] Figure 2 This is a physical picture of the orthogonal stacked energetic film of the present invention.

[0023] Figure 3 It is a SEM picture of the orthogonal stacked energetic film of the present invention.

[0024] Figure 4 This is a diagram showing the ignition condition of the orthogonal stacked energetic film of the present invention. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0026] Example 1

[0027] This embodiment is used to provide a 3D printing method for an orthogonal laminated energetic film for a solid rocket motor, which specifically includes the following steps:

[0028] Step 1: Preparation of dispersion solvent. Weigh 0.85g PVDF and 0.15g TPU in proportion and add them to 10g DMF, mix by ultrasonic for 30min, and stir for 45min to obtain dispersion solvent;

[0029] Step 2: Preparation of energetic ink: 0.85 g of nano titanium powder, 2.10 g of nano aluminum powder and 6.05 g of nano copper oxide powder were weighed in proportion and added to the dispersing solvent in step 1, and ultrasonically mixed for 30 min to fully mix the titanium powder, nano thermite and the dispersing solvent, and then the mixed solution was placed in a water bath magnetic stirrer and stirred for 12 h to obtain energetic ink;

[0030] Step 3: Preparation of energetic film. Use a vacuum pump to adsorb the plastic film onto the heating platform, load the prepared energetic ink into a disposable syringe of 5 ml, and fix it on the 3D motion platform. According to the required loading amount, control the X, Y, Z axes and the pressure plate above the syringe through computer software to push the ink evenly. Under the condition of controlling the printing line spacing, print the energetic ink on the plastic film in the form of alternating vertical and horizontal printing lines. The printing structure principle is as follows: Figure 1 As shown, the printed product is as follows Figure 2The ink pushing speed is 3.85 μL / s, the needle moving speed is 20 mm / s, and the energetic ink is cured at 55°C for 60 min to form an orthogonal laminated energetic film.

[0031] in, Figure 3 The SEM image of the prepared orthogonal laminated energetic film shows that there are dispersed granular morphologies on the surface of the film, indicating that the dispersant can be well wrapped on the surface of the nano-aluminum thermite particles to form a particle network structure.

[0032] Figure 4 The ignition diagram of the prepared orthogonal stacked energetic film is shown in Figure 1. As can be seen from the figure, the energetic film has a short ignition time and a fast burning speed.

[0033] Example 2

[0034] This embodiment is used to provide a 3D printing method for an orthogonal laminated energetic film for a solid rocket motor, which specifically includes the following steps:

[0035] Step 1: Preparation of dispersion solvent. Weigh 0.85g PVDF and 0.15g TPU in proportion and add them to 15g DMF, mix by ultrasonic for 30min, and stir for 45min to obtain dispersion solvent;

[0036] Step 2: Preparation of energetic ink: 0.85 g of nano titanium powder, 2.10 g of nano aluminum powder and 6.05 g of nano copper oxide powder were weighed in proportion and added to the dispersing solvent in step 1, and ultrasonically mixed for 30 min to fully mix the titanium powder, nano thermite and the dispersing solvent, and then the mixed solution was placed in a water bath magnetic stirrer and stirred for 12 h to obtain energetic ink;

[0037] Step 3: Preparation of energetic film. Use a vacuum pump to adsorb the plastic film onto the heating platform, load the prepared energetic ink into a disposable syringe of 5 ml, and fix it on a three-dimensional motion platform. According to the required loading amount, the computer software controls the X, Y, Z axes and the pressure plate above the syringe to push the ink evenly. While controlling the printing line spacing, print the energetic ink on the plastic film in the form of alternating vertical and horizontal printing lines. The ink pushing speed is 3.85 μL / s, the needle movement speed is 20 mm / s, and the energetic ink is cured at 55 ° C for 60 minutes to form an orthogonal laminated energetic film.

[0038] Example 3

[0039] This embodiment is used to provide a 3D printing method for an orthogonal laminated energetic film for a solid rocket motor, which specifically includes the following steps:

[0040] Step 1: Preparation of dispersion solvent. Weigh 0.85g PVDF and 0.15g TPU in proportion and add them to 12.3g DMF, mix by ultrasonic for 30min, and stir for 45min to obtain dispersion solvent;

[0041] Step 2: Preparation of energetic ink: 0.85 g of nano titanium powder, 2.10 g of nano aluminum powder and 6.05 g of nano copper oxide powder were weighed in proportion and added to the dispersing solvent in step 1, and ultrasonically mixed for 30 min to fully mix the titanium powder, nano thermite and the dispersing solvent, and then the mixed solution was placed in a water bath magnetic stirrer and stirred for 12 h to obtain energetic ink;

[0042] Step 3: Preparation of energetic film. Use a vacuum pump to adsorb the plastic film onto the heating platform, load the prepared energetic ink into a disposable syringe of 5 ml, and fix it on a three-dimensional motion platform. According to the required loading amount, the computer software controls the X, Y, Z axes and the pressure plate above the syringe to push the ink evenly. While controlling the printing line spacing, print the energetic ink on the plastic film in the form of alternating vertical and horizontal printing lines. The ink pushing speed is 3.85 μL / s, the needle movement speed is 20 mm / s, and the energetic ink is cured at 55 ° C for 60 minutes to form an orthogonal laminated energetic film.

[0043] Example 4

[0044] This embodiment is used to provide a 3D printing method for an orthogonal laminated energetic film for a solid rocket motor, which specifically includes the following steps:

[0045] Step 1: Preparation of dispersion solvent. Weigh 0.90g PVDF and 0.10g TPU according to the proportion and add them to 10g DMF, mix them by ultrasonic for 30min, and stir for 45min to obtain dispersion solvent;

[0046] Step 2: Preparation of energetic ink: 0.85 g of nano titanium powder, 2.10 g of nano aluminum powder and 6.05 g of nano copper oxide powder were weighed in proportion and added to the dispersing solvent in step 1, and ultrasonically mixed for 30 min to fully mix the titanium powder, nano thermite and the dispersing solvent, and then the mixed solution was placed in a water bath magnetic stirrer and stirred for 12 h to obtain energetic ink;

[0047] Step 3: Preparation of energetic film. Use a vacuum pump to adsorb the plastic film onto the heating platform, load the prepared energetic ink into a disposable syringe of 5 ml, and fix it on a three-dimensional motion platform. According to the required loading amount, the computer software controls the X, Y, Z axes and the pressure plate above the syringe to push the ink evenly. While controlling the printing line spacing, print the energetic ink on the plastic film in the form of alternating vertical and horizontal printing lines. The ink pushing speed is 3.85 μL / s, the needle movement speed is 20 mm / s, and the energetic ink is cured at 55 ° C for 60 minutes to form an orthogonal laminated energetic film.

[0048] Example 5

[0049] This embodiment is used to provide a 3D printing method for an orthogonal laminated energetic film for a solid rocket motor, which specifically includes the following steps:

[0050] Step 1: Preparation of dispersion solvent. Weigh 1.00 g PVDF and add it to 10 g DMF, mix by ultrasonic for 30 min, and stir for 45 min to obtain dispersion solvent;

[0051] Step 2: Preparation of energetic ink: 0.85 g of nano titanium powder, 2.10 g of nano aluminum powder and 6.05 g of nano copper oxide powder were weighed in proportion and added to the dispersing solvent in step 1, and ultrasonically mixed for 30 min to fully mix the titanium powder, nano thermite and the dispersing solvent, and then the mixed solution was placed in a water bath magnetic stirrer and stirred for 12 h to obtain energetic ink;

[0052] Step 3: Preparation of energetic film. Use a vacuum pump to adsorb the plastic film onto the heating platform, load the prepared energetic ink into a disposable syringe of 5 ml, and fix it on a three-dimensional motion platform. According to the required loading amount, the computer software controls the X, Y, Z axes and the pressure plate above the syringe to push the ink evenly. While controlling the printing line spacing, print the energetic ink on the plastic film in the form of alternating vertical and horizontal printing lines. The ink pushing speed is 3.85 μL / s, the needle movement speed is 20 mm / s, and the energetic ink is cured at 55 ° C for 60 minutes to form an orthogonal laminated energetic film.

Claims

1. A 3D printing method for orthogonally stacked energetic films, characterized in that: The steps include: Step (1): using N,N-dimethylformamide (DMF) as a solvent, polyvinylidene fluoride (PVDF) and thermoplastic polyurethane (TPU) as dispersants, ultrasonically mixing the three, stirring them evenly, and obtaining a mixed solution; Step (2): adding nano-thermite and nano-titanium powder to the mixed solution of step (1), and then performing ultrasonic mixing and stirring to obtain energetic ink; Step (3): Place the energetic ink prepared in step (2) into a 2-10 ml syringe, use a vacuum pump to adsorb the plastic film onto the heating platform, start the 3D printing device, print the energetic ink on the plastic film in an orthogonal stacking manner, and cure the energetic ink at 45-55° C. for 60-120 min to form an energetic film.

2. The method according to claim 1, characterized in that In step (1), the mass of poly(vinylidene fluoride) PVDF is 0.8-1.0 g, the mass of thermoplastic polyurethane TPU is 0-0.2 g, and the mass of solvent is 10-15 g.

3. The method according to claim 2, characterized in that The specific parameters of the ultrasonic mixing and stirring in step (1) are: ultrasonic mixing for 30-60 min, stirring for 30-60 min.

4. The method according to claim 3, characterized in that The mass ratio of the nano-thermite and nano-titanium powder added in step (2) is 9:1, the nano-thermite includes nano-aluminum powder and nano-copper oxide powder, the mass ratio of the nano-aluminum powder and the nano-copper oxide powder is 1:3, and the added amount of the nano-aluminum powder is 1.9-2.1g.

5. The method according to claim 4, characterized in that In step (2), stir for 12±2h.

6. The method according to claim 5, characterized in that The 3D printing device used in step (3) includes a three-dimensional motion platform and an MC600 motion controller.

7. The method according to claim 6, characterized in that In step (3), the ink is injected onto the plastic film at an ink pushing speed of 0.77 μL / s-3.85 μL / s, and the needle movement speed is 5 mm / s-20 mm / s.

8. The method according to claim 7, characterized in that The orthogonal lamination method in step (3) is specifically as follows: the printing directions of adjacent layers are perpendicular to each other while controlling the spacing.

9. An orthogonal laminated energetic film, characterized in that: The method is prepared by any one of claims 1 to 8.

Citation Information

Patent Citations

  • Flexible energetic materials and related methods

    US20170137337A1

  • Conductive ink composition and article of manufacture made therefrom

    US20200354600A1

  • Method for preparing polyvinylidene fluoride-coated micro-nano aluminum powder

    WO2021036679A1