Preparation method of sodium ion battery Prussian white positive electrode material

The Prussian white cathode material for sodium ion batteries is prepared by a liquid-liquid reaction method, which solves the problem of poor performance of Prussian white cathode materials in the existing technology, achieves high cycle stability and rate performance, and reduces production costs.

CN118724014APending Publication Date: 2024-10-01WUHAN UNIV OF TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310318745.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing Prussian white cathode material for sodium-ion batteries has poor cycle performance and rate performance, mainly due to structural defects and crystallization water problems that cause the framework to be unstable, and the co-precipitation method using solid-liquid reaction is complex and non-uniform, which affects the material's performance. performance.

Method used

The liquid-liquid reaction method is used to prepare the Prussian white cathode material for sodium ion batteries by co-precipitating sodium cyanide and soluble divalent transition metal salts at a certain reaction temperature and time, and using organic acid sodium salts and pH regulators to regulate the reaction. speed and crystallinity, reducing the vacancies and crystal water content in the structure.

Benefits of technology

Significantly improved the cycle stability and rate performance of the Prussian white cathode material for sodium-ion batteries. The capacity retention rate after 600 cycles at 1C reached 81.6%, and the specific capacity at 10C was 90.5mAh/g, which reduced production costs and improved improve material uniformity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724014A_ABST
    Figure CN118724014A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a sodium ion battery Prussian white positive electrode material, and belongs to the technical field of sodium ion batteries. The preparation method comprises the following steps: dissolving sodium cyanide in deionized water to prepare a solution A; dissolving a soluble divalent transition metal salt, an organic acid sodium salt and a pH regulator in deionized water to prepare a solution B; mixing the solution A and the solution B or slowly dropwise adding the solution A and the solution B into the solution C at the same time, and carrying out coprecipitation reaction at a certain reaction temperature for a certain reaction time to prepare a solid precipitate; the solution C is deionized water or a sodium salt solution; and finally, centrifuging, washing and vacuum-drying the obtained solid precipitate to obtain the sodium ion battery Prussian white positive electrode material. The capacity retention ratio of the positive electrode material is up to 81.6% after the positive electrode material is circulated for 600 circles under the current of 1C, the specific capacity is 90.5 mAh / g under the current of 10C, and the positive electrode material shows excellent cycling stability and rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a method for preparing a Prussian white positive electrode material for a sodium ion battery. Background Art

[0002] Lithium-ion batteries are widely used in energy storage devices due to their high energy density and long cycle life. However, lithium resources are unevenly distributed and have low abundance, which cannot meet the rapidly growing energy storage needs of society. Therefore, it is urgent to develop new battery technologies to replace lithium-ion batteries. Sodium-ion batteries have potential advantages in large-scale energy storage due to their high sodium abundance, low cost and high safety, and are expected to become a new generation of energy storage batteries.

[0003] At present, the cathode materials of sodium ion batteries mainly include phosphates, transition metal oxides, Prussian blue analogs, etc. Prussian blue analogs (PBAs) have attracted attention due to their non-toxicity, simple synthesis process, low cost and high discharge voltage. Their three-dimensional framework structure and large ion channels allow Na + Fast deintercalation and low lattice strain capability are widely considered to be promising cathode materials for sodium-ion batteries. However, due to the rapid precipitation reaction, Fe(CN)6 vacancies are easily generated in the PBA framework during the synthesis process. The presence of vacancies reduces the cycle stability and rate performance of the material, and reduces the Na + Therefore, it is urgent to explore the synthesis of sodium-rich Prussian blue analogs as cathode materials.

[0004] Prussian white (PW) cathode material is a Prussian blue analogue, a fully reduced and sodiumized form of Prussian blue, containing high sodium. Due to its low cost and high theoretical energy density, it is a highly potential cathode material for sodium-ion batteries. Prussian white cathode materials have technical bottlenecks in their preparation process, mainly due to structural defects and crystal water problems, which lead to poor cycle performance and rate performance of Prussian white cathode materials.

[0005] The prior art has explored the preparation of Prussian white (PW) positive electrode materials.

[0006] You used Na4Fe(CN)6·10H2O as raw material to synthesize highly crystalline Na 0.61 Fe[Fe(CN)6] 0.94 (DOI:10.1039 / c3ee44004d), as a positive electrode material for sodium-ion batteries, it exhibits high cycle stability, but the Na component contains only 0.61 per unit, which limits the theoretical capacity of the full battery.

[0007] Jiang synthesized Na using Na4Fe(CN)6·10H2O as raw material.0.65 Fe[Fe(CN)6] 0.93 (DOI:10.1002 / adfm.201600747), although it exhibits good rate performance and cycle stability, it also suffers from the problem of low Na component, containing 0.65 per unit.

[0008] At present, some high-Na component PBAs have also been reported. For example, Wu synthesized Na4Fe(CN)6·10H2O and CoCl2 as raw materials. 1.85 Co[Fe(CN)6] 0.99 (DOI:10.1021 / acsami.5b12620); Yang synthesized Na using Na4Fe(CN)6·10H2O and FeCl2 as raw materials. 1.73 Fe[Fe(CN)6] 0.98 (DOI:10.1149 / 2.0031610jes); Although it has a high Na content, the low crystallinity of the Prussian white positive electrode material causes the framework to collapse and become unstable during the charge and discharge process.

[0009] Therefore, exploring the preparation of Prussian white positive electrode materials with high sodium content and excellent cycle performance and rate performance is one of the research focuses.

[0010] Prior art CN115650254A provides a raw material pre-type iron-based Prussian blue analog and a preparation method thereof, wherein sodium cyanide is used as a complexing cyanide source, reduced iron powder is used as an iron source, sodium citrate is used as a complexing agent and a supplementary sodium source, and a Prussian blue analog is directly synthesized by a coprecipitation method; the discharge capacity reaches 118 mAh / g under the charge-discharge curve at 0.1C; after 200 cycles at 1C, the capacity remains at 108 mAh / g, and the capacity retention rate is 98.1%. However, using reduced iron powder as the source of metal ions, the coprecipitation reaction is a solid-liquid reaction (a reaction between a solid and a liquid), and the influencing factors of the solid-liquid reaction are relatively complex. On the one hand, the specific gravity of the metal powder is greater than the specific gravity of the liquid, and it is easy to precipitate, and the coprecipitation reaction is not uniform; on the other hand, the reaction rate of the solid-liquid reaction involves the chemical reaction of the interface, the concentration of the liquid phase reactant and the crystal surface structure, and the process control of the coprecipitation reaction is relatively strict and complex, and the cycle performance stability of the prepared sodium ion battery Prussian white positive electrode material is relatively poor.

[0011] Therefore, exploring the preparation of Prussian white positive electrode materials with high sodium content and excellent cycle performance and rate performance remains an important and arduous issue. Summary of the invention

[0012] In order to solve the above technical problems, in a first aspect, the present invention provides a method for preparing a Prussian white positive electrode material for a sodium ion battery, comprising the following steps:

[0013] S1. Preparation of solution A: dissolving sodium cyanide in deionized water to prepare solution A;

[0014] S2. Preparation of solution B: dissolving a soluble divalent transition metal salt, an organic acid sodium salt and a pH adjuster in deionized water to prepare solution B;

[0015] S3, mixing solution A prepared in step S1 with solution B prepared in step S2 or slowly dropping solution A and solution B into solution C at the same time, and performing a coprecipitation reaction at a certain reaction temperature and reaction time to prepare a solid precipitate; solution C is deionized water or a sodium salt solution;

[0016] S4. Centrifuge, wash and dry the solid precipitate prepared in S3 to obtain a Prussian white positive electrode material for a sodium ion battery.

[0017] The concentration of sodium cyanide in step S1 solution A is 0.05-1 mol / L;

[0018] In step S2, the concentration of the divalent transition metal salt in solution B is 0.05 to 1 mol / L; the molar ratio of the divalent transition metal salt to the organic acid sodium salt in solution B is 1:1 to 1:10;

[0019] The soluble divalent transition metal salt in step S2 is at least one of copper nitrate, nickel nitrate, manganese nitrate, cobalt nitrate, zinc nitrate, nickel acetate, manganese acetate, zinc acetate, copper sulfate, nickel sulfate, ferrous sulfate, zinc sulfate, manganese sulfate, ferrous chloride, nickel chloride, copper chloride, cobalt chloride and zinc chloride; the organic acid sodium salt is at least one of sodium ethylenediaminetetraacetate, sodium citrate, sodium ascorbate, sodium tartrate and sodium lactate;

[0020] In some embodiments, preferably, the soluble divalent transition metal salt is ferrous sulfate; the organic acid sodium salt is sodium citrate;

[0021] The organic acid sodium salt plays a chelating role in the preparation system, which can effectively control the synthesis reaction rate of the Prussian white positive electrode material of the sodium ion battery; regulate the crystallinity of the material; adjust the sodium content in the material, and reduce the vacancies and crystal water content in the structure.

[0022] The pH regulator in step S2 is at least one of ascorbic acid, sodium carbonate, citric acid and sodium hydroxide; the pH regulator adjusts the pH of solution B to 5.5-7.5;

[0023] The role of the pH regulator in the preparation system is to control the crystallization process in the coprecipitation reaction and adjust the size of the crystal particles.

[0024] In some embodiments, preferably, the pH adjuster is citric acid;

[0025] In step S3, the mixing method of solution A and solution B is that solution A is slowly dropped into solution B or solution B is slowly dropped into solution A; the mixing rate is 0.05 - 0.6 mL / min;

[0026] In step S3, solution A and solution B are respectively and simultaneously slowly dropped into solution C, and the dropping rate is 0.05 - 0.6 mL / min;

[0027] When solution C is a sodium salt solution in step S3, the concentration of the sodium salt is 0.05 - 1 mol / L; the sodium salt is at least one of sodium ethylenediaminetetraacetate, sodium citrate, sodium ascorbate, sodium tartrate, sodium lactate, sodium chloride, sodium sulfate, and sodium acetate;

[0028] In some embodiments, preferably, solution C is a sodium acetate solution;

[0029] In step S3, the co - precipitation reaction temperature is 25 - 80 °C, and the co - precipitation reaction time is 12 - 48 h;

[0030] In step S4, the washing solvent is deionized water and absolute ethanol; the drying condition is vacuum drying, the drying temperature is 60 - 120 °C, and the drying time is 10 - 24 h.

[0031] In the second aspect, the present invention provides a sodium - ion battery Prussian white cathode material, which is prepared by the preparation method of the sodium - ion battery Prussian white cathode material in the first aspect. The structural general formula of the sodium - ion battery Prussian white cathode material is Na X M[Fe(CN)6]y·nH2O, where M is a transition metal element, 0 < x ≤ 2, 0 < y ≤ 1, 0 < n ≤ 2; the transition metal element comes from the metal ions of divalent transition metal salts.

[0032] In the third aspect, the present invention provides a positive electrode sheet, and the positive electrode material of the positive electrode sheet is the sodium - ion battery Prussian white cathode material prepared by the preparation method in the first aspect or the sodium - ion battery Prussian white cathode material in the second aspect.

[0033] In the fourth aspect, the present invention provides a sodium - ion battery, and the positive electrode material of the sodium - ion battery is the sodium - ion battery Prussian white cathode material prepared by the preparation method in the first aspect or the sodium - ion battery Prussian white cathode material in the second aspect.

[0034] The sodium - ion battery Prussian white cathode material prepared by the present invention has a high sodium content. It cycles 600 times at a current of 1C, and the capacity retention rate is as high as 81.6%; at a current of 10C, the specific capacity is 90.5 mAh / g, and the cycle stability and rate performance are significantly improved.

[0035] In the process of preparing the positive electrode material of the sodium ion battery, the present invention adopts sodium cyanide, which reduces the production cost compared with the sodium ferrocyanide decahydrate commonly used in the prior art.

[0036] The present invention adopts a soluble divalent transition metal salt as a source of metal ions, dissolves the soluble divalent transition metal salt in deionized water, and the coprecipitation reaction is a liquid-liquid reaction (a reaction between liquids). The reaction system is a uniform solution. Compared with the prior art that adopts metal powder as a source of metal ions, the coprecipitation reaction is a solid-liquid reaction (a reaction between a solid and a liquid). The present invention has good coprecipitation efficiency and crystallization effect. Therefore, the prepared sodium ion battery Prussian white positive electrode material has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The present disclosure will be further described in detail below in conjunction with the accompanying drawings and preferred embodiments, but those skilled in the art will appreciate that these drawings are drawn only for the purpose of explaining the preferred embodiments and therefore should not be used as a limitation on the scope of the present disclosure. In addition, unless otherwise specified, the drawings are only schematically representing the composition or structure of the described objects and may contain exaggerated displays, and the drawings are not necessarily drawn to scale.

[0038] Figure 1 Schematic diagram of the preparation method of Prussian white positive electrode material for sodium ion batteries;

[0039] Figure 2 X-ray diffraction pattern of the Prussian white positive electrode material for sodium ion batteries prepared in Example 1-3;

[0040] Figure 3 X-ray diffraction patterns of the sodium ion battery Prussian white positive electrode materials prepared in Comparative Examples 1-3

[0041] Figure 4 Scanning electron microscope image of the Prussian white positive electrode material for sodium ion battery prepared in Example 1;

[0042] Figure 5 Voltage specific capacity curve of the Prussian white positive electrode material for sodium ion batteries prepared in Example 1;

[0043] Figure 6 Cycling performance diagram of the sodium ion battery Prussian white positive electrode material prepared in Example 1 and Comparative Example 1;

[0044] Figure 7 Rate performance diagram of the Prussian white positive electrode material for sodium ion batteries prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0045] The following is combined with Figures 1 to 7 , a detailed description of the present disclosure is given.

[0046] In order to make the purpose, technical solution and advantages of the present disclosure more clear, the present disclosure is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the present disclosure.

[0047] The present invention provides a method for preparing a sodium ion battery Prussian white positive electrode material, such as Figure 1 As shown, the following steps are included:

[0048] S1. Preparation of solution A: dissolving sodium cyanide in deionized water to prepare solution A;

[0049] S2. Preparation of solution B: dissolving a soluble divalent transition metal salt, an organic acid sodium salt and a pH adjuster in deionized water to prepare solution B;

[0050] S3, mixing solution A prepared in step S1 with solution B prepared in step S2 or slowly dropping solution A and solution B into solution C at the same time, and performing a coprecipitation reaction at a certain reaction temperature and reaction time to prepare a solid precipitate; solution C is deionized water or a sodium salt solution;

[0051] S4. Centrifuge, wash and dry the solid precipitate prepared in S3 to obtain a Prussian white positive electrode material for a sodium ion battery.

[0052] The concentration of sodium cyanide in step S1 solution A is 0.05-1 mol / L;

[0053] In step S2, the concentration of the divalent transition metal salt in solution B is 0.05 to 1 mol / L; the molar ratio of the divalent transition metal salt to the organic acid sodium salt in solution B is 1:1 to 1:10;

[0054] The soluble divalent transition metal salt in step S2 is at least one of copper nitrate, nickel nitrate, manganese nitrate, cobalt nitrate, zinc nitrate, nickel acetate, manganese acetate, zinc acetate, copper sulfate, nickel sulfate, ferrous sulfate, zinc sulfate, manganese sulfate, ferrous chloride, nickel chloride, copper chloride, cobalt chloride and zinc chloride; the organic acid sodium salt is at least one of sodium ethylenediaminetetraacetate, sodium citrate, sodium ascorbate, sodium tartrate and sodium lactate;

[0055] Preferably, the soluble divalent transition metal salt is ferrous sulfate; the organic acid sodium salt is sodium citrate;

[0056] The organic acid sodium salt plays a chelating role in the preparation system, which can effectively control the synthesis reaction rate of the Prussian white positive electrode material of the sodium ion battery; regulate the crystallinity of the material; adjust the sodium content in the material, and reduce the vacancies and crystal water content in the structure.

[0057] The pH regulator in step S2 is at least one of ascorbic acid, sodium carbonate, citric acid and sodium hydroxide; the pH regulator adjusts the pH of solution B to 5.5-7.5;

[0058] The role of the pH regulator in the preparation system is to control the crystallization process in the coprecipitation reaction and adjust the size of the crystal particles.

[0059] Preferably, the pH adjuster is citric acid;

[0060] In step S3, solution A and solution B are mixed by slowly dropping solution A into solution B or slowly dropping solution B into solution A; the mixing rate is 0.05-0.6 mL / min;

[0061] In step S3, solution A and solution B are slowly added to solution C simultaneously, and the dropping rate is 0.05-0.6 mL / min;

[0062] When solution C in step S3 is a sodium salt solution, the concentration of the sodium salt is 0.05-1 mol / L; the sodium salt is at least one of sodium ethylenediaminetetraacetate, sodium citrate, sodium ascorbate, sodium tartrate, sodium lactate, sodium chloride, sodium sulfate and sodium acetate;

[0063] Preferably, solution C is a sodium acetate solution;

[0064] In step S3, the coprecipitation reaction temperature is 25 to 80° C., and the coprecipitation reaction time is 12 to 48 hours;

[0065] In step S4, the washing solvent is deionized water and anhydrous ethanol; the drying condition is vacuum drying, the drying temperature is 60-120° C., and the drying time is 10-24 hours.

[0066] Example 1

[0067] Sodium cyanide was dissolved in a certain amount of deionized water to obtain a concentration of 0.3 mol L -1 Solution A;

[0068] Dissolve ferrous sulfate heptahydrate in a certain amount of deionized water to obtain a concentration of 0.1 mol L -1 Solution B, adding sodium citrate and citric acid to solution B, wherein the molar ratio of sodium citrate to ferrous sulfate heptahydrate is 7:1, and adding citric acid to adjust the pH to 6.5;

[0069] Solution A was slowly added dropwise to solution B at a dropping rate of 0.3 mL / min, and a suspension was obtained by coprecipitation reaction at 30°C. The suspension was aged at this temperature for 24 h to obtain a solid precipitate;

[0070] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 80° C. in vacuum for 24 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0071] The sodium ion battery Prussian white positive electrode material prepared in Example 1 was subjected to X-ray diffraction analysis (eg Figure 2 As shown), ICP (inductively coupled plasma spectroscopy) analysis, scanning electron microscopy (as shown Figure 4 as shown) and voltage ratio detection (as shown Figure 5 shown).

[0072] Figure 2 The sodium ion battery Prussian white positive electrode material prepared in Example 1 is presented. Figure 2 It can be seen that the product structure of Example 1 is a sodium-rich monoclinic phase.

[0073] Combined with the ICP analysis results of the sodium ion battery Prussian white positive electrode material prepared in Example 1, the molecular formula of the sodium ion battery Prussian white positive electrode material prepared in Example 1 is Na 1.77 There are 1.77 Na in a Fe[Fe(CN)6],1 molecule. Therefore, the sodium ion battery Prussian white positive electrode material prepared in Example 1 is a sodium-rich Prussian white positive electrode material.

[0074] Figure 4 This is a scanning electron microscope image of the Prussian white positive electrode material for a sodium ion battery prepared in Example 1. Figure 4 It can be seen that the product of Example 1 is in the form of secondary cubic particles, with primary particles of about 2 μm and secondary particles of about 6 μm.

[0075] Figure 5 This is a voltage-to-capacity curve of the sodium-ion battery Prussian white positive electrode material prepared in Example 1. When the current size is 0.3C, the product prepared in Example 1 has a first-cycle discharge specific capacity of 123.2mAh / g; a second-cycle discharge specific capacity of 116.4mAh / g; and a third-cycle discharge specific capacity of 114.6mAh / g. The first-cycle discharge specific capacity is higher than the second-cycle, so it is further explained that the sodium-ion battery Prussian white positive electrode material prepared in Example 1 is a sodium-rich Prussian white positive electrode material.

[0076] The specific capacity of the sodium ion battery Prussian white positive electrode material prepared in Example 1 was also tested at currents of 0.1C and 10C, respectively. The specific capacity at a current of 0.1C was 137.1 mAh / g; the specific capacity at a current of 10C was 90.5 mAh / g.

[0077] The capacity retention rate of the sodium ion battery Prussian white positive electrode material prepared in Example 1 after 500 cycles at a current of 1C is 83.3%.

[0078] Example 2

[0079] Sodium cyanide was dissolved in a certain amount of deionized water to obtain a concentration of 0.5 mol L -1 Solution A;

[0080] Dissolve ferrous sulfate heptahydrate in a certain amount of deionized water to obtain a concentration of 0.4 mol L -1 Solution B, adding sodium citrate and citric acid to solution B, wherein the molar ratio of sodium citrate to ferrous sulfate heptahydrate is 4.5:1, and adding citric acid to adjust the pH to 6.9;

[0081] Solution B was slowly added dropwise to solution A at a dropping rate of 0.2 mL / min, and a suspension was obtained by coprecipitation reaction at 50°C. The suspension was aged at this temperature for 24 h to obtain a solid precipitate;

[0082] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 80° C. in vacuum for 16 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0083] The Prussian white positive electrode material for sodium ion battery prepared in Example 2 was subjected to X-ray diffraction analysis. Figure 2 As shown, the product structure of Example 2 is a sodium-rich monoclinic phase.

[0084] Combined with the ICP analysis results of the sodium ion battery Prussian white positive electrode material prepared in Example 2, the molecular formula of the sodium ion battery Prussian white positive electrode material prepared in Example 2 is Na 1.68 Fe[Fe(CN)6] contains 1.68 Na in one molecule. Therefore, the sodium ion battery Prussian white positive electrode material prepared in Example 2 is a sodium-rich Prussian white positive electrode material.

[0085] Example 3

[0086] Sodium cyanide was dissolved in a certain amount of deionized water to obtain a concentration of 0.3 mol L -1 Solution A;

[0087] Dissolve ferrous sulfate heptahydrate in a certain amount of deionized water to obtain a concentration of 0.6 mol L -1 Solution B, sodium citrate and citric acid are added to solution B, wherein the molar ratio of sodium citrate to ferrous sulfate heptahydrate is 6:1, and citric acid is added to adjust the pH to 6.0; solution A and solution B are slowly added dropwise to solution C at the same time, wherein the dropwise acceleration rate is 0.1 mL / min, solution C is a sodium acetate solution with a concentration of 0.2 mol / L, a suspension is obtained by coprecipitation reaction at 60°C, and the suspension is aged at this temperature for 36 hours to obtain a solid precipitate;

[0088] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 100° C. in vacuum for 24 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0089] X-ray diffraction analysis was performed on the sodium ion battery Prussian white positive electrode material prepared in Example 3. Figure 2 As shown, the product structure of Example 3 is a sodium-rich monoclinic phase.

[0090] Combined with the ICP analysis results of the sodium ion battery Prussian white positive electrode material prepared in Example 3, the molecular formula of the sodium ion battery Prussian white positive electrode material prepared in Example 3 is Na 1.73 Fe[Fe(CN)6] contains 1.73 Na in one molecule. Therefore, the sodium ion battery Prussian white positive electrode material prepared in Example 3 is a sodium-rich Prussian white positive electrode material.

[0091] Comparative Example 1

[0092] Sodium ferrocyanide decahydrate was dissolved in a certain amount of deionized water to obtain a concentration of 0.3 mol L -1 Solution A;

[0093] Dissolve ferrous sulfate heptahydrate in a certain amount of deionized water to obtain a concentration of 0.1 mol L -1 Solution B, adding sodium citrate and citric acid to solution B, wherein the molar ratio of sodium citrate to ferrous sulfate heptahydrate is 7:1, and adding citric acid to adjust the pH to 6.5;

[0094] Solution A was slowly added dropwise to solution B at a dropping rate of 0.3 mL / min, and a suspension was obtained by coprecipitation reaction at 30°C. The suspension was aged at this temperature for 24 h to obtain a solid precipitate;

[0095] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 80° C. in vacuum for 24 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0096] The sodium ion battery Prussian white positive electrode material prepared in Comparative Example 1 was subjected to X-ray diffraction analysis (eg Figure 3 As shown) and ICP (inductively coupled plasma spectroscopy) analysis.

[0097] Figure 3 The X-ray diffraction pattern of the Prussian white positive electrode material for sodium ion battery prepared in Comparative Example 1 is presented. Figure 3 It can be seen that the product structure of Comparative Example 1 is a sodium-rich monoclinic phase. Combined with the ICP results of the product of Comparative Example 1, the molecular formula of the product is Na 1.52 Fe[Fe(CN)6].

[0098] Comparative Example 2

[0099] Sodium ferrocyanide decahydrate was dissolved in a certain amount of deionized water to obtain a concentration of 0.5 mol L -1 Solution A;

[0100] Dissolve ferrous sulfate heptahydrate in a certain amount of deionized water to obtain a concentration of 0.4 mol L -1 Solution B, adding sodium citrate and citric acid to solution B, wherein the molar ratio of sodium citrate to ferrous sulfate heptahydrate is 4.5:1, and adding citric acid to adjust the pH to 6.9;

[0101] Solution B was slowly added dropwise to solution A at a dropping rate of 0.2 mL / min, and a suspension was obtained by coprecipitation reaction at 50°C. The suspension was aged at this temperature for 24 h to obtain a solid precipitate;

[0102] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 80° C. in vacuum for 16 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0103] X-ray diffraction analysis was performed on the sodium ion battery Prussian white positive electrode material prepared in Comparative Example 2 (eg Figure 3 shown) analysis.

[0104] Figure 3 The X-ray diffraction pattern of the Prussian white positive electrode material prepared in Comparative Example 2 is presented. Figure 3 It can be seen that the product structure of Comparative Example 2 is a sodium-rich monoclinic phase.

[0105] Comparative Example 3

[0106] Sodium ferrocyanide decahydrate was dissolved in a certain amount of deionized water to obtain a concentration of 0.3 mol L -1 Solution A;

[0107] Dissolve ferrous sulfate heptahydrate in a certain amount of deionized water to obtain a concentration of 0.6 mol L -1 Solution B, adding sodium citrate and citric acid to solution B, wherein the molar ratio of sodium citrate to ferrous sulfate heptahydrate is 6:1, and adding citric acid to adjust the pH to 6.0;

[0108] Solution A and solution B are slowly added dropwise to solution C at the same time, wherein the dropping rate is 0.1 mL / min, solution C is a sodium acetate solution, and the concentration is 0.2 mol / L, and a suspension is obtained by coprecipitation reaction at 60°C, and the suspension is aged at this temperature for 36 hours to obtain a solid precipitate;

[0109] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 100° C. in vacuum for 24 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0110] X-ray diffraction analysis was performed on the sodium ion battery Prussian white positive electrode material prepared in Comparative Example 3 (eg Figure 3 shown) analysis.

[0111] Figure 3 The X-ray diffraction pattern of the Prussian white positive electrode material prepared in Comparative Example 3 is presented. Figure 3 It can be seen that the product structure of Comparative Example 3 is a sodium-rich monoclinic phase.

[0112] Comparative Example 4

[0113] Sodium cyanide was dissolved in a certain amount of deionized water to obtain a concentration of 0.2 mol L -1 Solution A;

[0114] Add iron powder to a certain amount of deionized water, then add sodium citrate and citric acid to obtain a mixed solution B, wherein the molar ratio of sodium citrate to iron powder is 5:1, and citric acid is added to adjust the pH to 6.8;

[0115] Solution A was slowly added dropwise to solution B at a dropping rate of 0.6 mL / min, and a suspension was obtained by coprecipitation reaction at 30°C. The suspension was aged at this temperature for 24 h to obtain a solid precipitate;

[0116] The solid precipitate was centrifuged and washed three times with water and anhydrous ethanol; the product was dried at 100° C. in vacuum for 24 h to obtain the Prussian white positive electrode material for sodium ion batteries.

[0117] The Prussian white positive electrode material prepared in Comparative Example 4 was characterized by X-ray diffraction, and the results showed that the obtained product was a monoclinic Prussian white positive electrode material.

[0118] The electrochemical properties of the Prussian white positive electrode material prepared in Comparative Example 4 were tested. The results showed that when the current was 0.3C, the first-cycle discharge capacity was 106.2 mAh / g; when the current was 1C, the capacity retention rate was 62.4% after 500 cycles, and the capacity retention rate at a high rate of 10C was 63.8%.

[0119] The specific capacity, cycle stability and rate performance of the sodium ion battery Prussian white positive electrode material prepared with iron powder as the iron source in Comparative Example 4 are significantly reduced compared with the Prussian white positive electrode material prepared with ferrous sulfate as the iron source in Example 1. Therefore, using ferrous sulfate as the iron source is better than using iron powder as the iron source.

[0120] The present invention respectively tests the cycle performance of the sodium ion battery Prussian white positive electrode material prepared in Example 1 and Comparative Example 1. Figure 6As shown, the positive electrode material prepared in Example 1 has a specific capacity of 88.5 mAh / g after 600 cycles at a current of 1C, and a capacity retention rate of 81.6%; the positive electrode material prepared in Comparative Example 1 has a specific capacity of 47.2 mAh / g after 247 cycles at a current of 1C, and a capacity retention rate of 43.1%; the cycle stability of the positive electrode material prepared in Example 1 far exceeds the cycle stability of the positive electrode material prepared in Comparative Example 1, and the cycle stability of the positive electrode material prepared in Example 1 is significantly enhanced.

[0121] The present invention also carried out rate performance testing on the sodium ion battery Prussian white positive electrode materials prepared in Example 1 and Comparative Example 1, respectively. Figure 7 As shown, the capacity retention rate of the positive electrode material prepared in Example 1 is 74.1% at a current of 10C; the capacity retention rate of the positive electrode material prepared in Comparative Example 1 is 67.9% at a current of 10C; the rate performance of the positive electrode material prepared in Example 1 is greatly improved compared with the rate performance of the positive electrode material prepared in Comparative Example 1.

[0122] The present disclosure is described in detail above. The principles and implementation methods of the present disclosure are described in detail using specific examples in the present disclosure. The description of the above embodiments is only used to help understand the present disclosure and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present disclosure, several improvements and modifications can be made to the present disclosure, and these improvements and modifications also fall within the scope of protection of the claims of the present disclosure.

Claims

1. A method for preparing a sodium ion battery Prussian white positive electrode material, characterized in that: The steps include: S1. Preparation of solution A: dissolving sodium cyanide in deionized water to prepare solution A; S2. Preparation of solution B: dissolving a soluble divalent transition metal salt, an organic acid sodium salt and a pH adjuster in deionized water to prepare solution B; S3, mixing solution A prepared in step S1 with solution B prepared in step S2 or slowly dropping solution A and solution B into solution C at the same time, and performing a coprecipitation reaction at a certain reaction temperature and reaction time to prepare a solid precipitate; solution C is deionized water or a sodium salt solution; S4. Centrifuge, wash and dry the solid precipitate prepared in S3 to obtain a Prussian white positive electrode material for a sodium ion battery.

2. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: The concentration of sodium cyanide in solution A is 0.05-1 mol / L.

3. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: The concentration of the divalent transition metal salt in solution B is 0.05-1 mol / L; the molar ratio of the divalent transition metal salt to the organic acid sodium salt in solution B is 1:1-1:

10.

4. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: The soluble divalent transition metal salt in step S2 is at least one of copper nitrate, nickel nitrate, manganese nitrate, cobalt nitrate, zinc nitrate, nickel acetate, manganese acetate, zinc acetate, copper sulfate, nickel sulfate, ferrous sulfate, zinc sulfate, manganese sulfate, ferrous chloride, nickel chloride, copper chloride, cobalt chloride and zinc chloride; the organic acid sodium salt is at least one of sodium ethylenediaminetetraacetate, sodium citrate, sodium ascorbate, sodium tartrate and sodium lactate.

5. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: The pH adjuster in step S2 is at least one of ascorbic acid, sodium carbonate, citric acid and sodium hydroxide; the pH adjuster adjusts the pH of solution B to 5.5-7.

5.

6. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step S3, solution A and solution B are mixed in a manner of slowly dropping solution A into solution B or slowly dropping solution B into solution A; the mixing rate is 0.05-0.6 mL / min.

7. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step S3, solution A and solution B are respectively and simultaneously slowly added dropwise to solution C, with a dropping rate of 0.05-0.6 mL / min.

8. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: When solution C in step S3 is a sodium salt solution, the concentration of the sodium salt is 0.05-1 mol / L; the sodium salt is at least one of sodium edetate, sodium citrate, sodium ascorbate, sodium tartrate, sodium lactate, sodium chloride, sodium sulfate and sodium acetate.

9. The method for preparing the Prussian white positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step S3, the coprecipitation reaction temperature is 25-80° C., and the coprecipitation reaction time is 12-48 hours; in step S4, the washing solvent is deionized water and anhydrous ethanol; the drying condition is vacuum drying, the drying temperature is 60-120° C., and the drying time is 10-24 hours.

10. A sodium ion battery Prussian white positive electrode material, prepared by the preparation method of a sodium ion battery Prussian white positive electrode material according to any one of claims 1 to 9, characterized in that: The structural general formula of the Prussian white cathode material for the sodium-ion battery is Na X M[Fe(CN)6]y·nH2O, where M is a transition metal element, 0 < x ≤ 2, 0 < y ≤ 1, 0 < n ≤ 2; the transition metal element comes from the metal ions of divalent transition metal salts.

11. A positive electrode sheet, characterized in that: The positive electrode material of the positive electrode sheet is the sodium ion battery Prussian white positive electrode material prepared by the preparation method of any one of claims 1 to 9 or the sodium ion battery Prussian white positive electrode material according to claim 10.

12. A sodium ion battery, characterized in that: The positive electrode material of the sodium ion battery is the Prussian white positive electrode material of the sodium ion battery prepared by the preparation method of any one of claims 1 to 9 or the Prussian blue analog sodium ion battery positive electrode material according to claim 10.

Citation Information

Patent Citations

  • Prussian blue material, and preparation method and application thereof

    CN110921681A

  • Low-moisture-content Prussian blue sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery

    CN115023829A

  • Preparation method and application of Prussian blue sodium ion battery positive electrode material

    CN115611296A

  • Raw material preposed iron-based prussian blue analogue and preparation method thereof

    CN115650254A