Basic sodium ferrous sulfate positive electrode material as well as preparation method and application thereof

Preparation of alkaline sodium ferrous sulfate positive electrode material by high temperature and high pressure hydrothermal method has solved the problems of cumbersome synthesis route and high energy consumption in the prior art, improved the sodium content and compaction density of the material, and realized high-performance positive electrode material preparation.

CN119008936APending Publication Date: 2024-11-22HUBEI WANRUN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196618.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing synthetic route of using chlorophyllium ferrous sulfate positive electrode materials is complicated and has high energy consumption, and the sodium content of the prepared sodium ferrous sulfate positive electrode materials is low.

Method used

Using high-temperature and high-pressure hydrothermal method, slurry yellow sodium ferrous sulfate and urea is mixed and slurry, and alkaline sodium ferrous sulfate positive electrode material is generated through hydrothermal reaction, which avoids the traditional sintering process and increases the sodium content and compaction density. And by controlling the particle size, molar ratio and reaction conditions, the efficient preparation of the material is ensured.

Benefits of technology

The preparation of high-performance alkaline sodium ferrous sulfate positive electrode material has been achieved, with higher sodium content, larger capacity, higher compaction density, relatively high voltage, and lower process energy consumption, which is suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008936A_ABST
    Figure CN119008936A_ABST
Patent Text Reader

Abstract

The invention provides a basic sodium ferrous sulfate positive electrode material as well as a preparation method and application thereof, and belongs to the field of sodium batteries. Wherein the structural formula of the basic sodium ferrous sulfate positive electrode material is Na8Fe6 (SO4) 4 (OH) 12; the compaction density of the basic sodium ferrous sulfate positive electrode material is 2.2-2.3 g / mL, the BET specific surface area is 3-6 m < 2 > / g, and the powder resistivity is greater than 60 omega.cm. The basic sodium ferrous sulfate positive electrode material prepared by the invention has the advantages of higher sodium content, higher capacity, higher compaction density, higher voltage and excellent performance, and the preparation method is simple and suitable for industrial popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium batteries, and in particular to a basic sodium ferrous sulfate positive electrode material and a preparation method and application thereof. Background Art

[0002] Alluaudite-type sodium ferrous sulfate positive electrode material has a high operating voltage of 3.8V and can provide excellent energy density compared to other polyanion positive electrode materials. However, the crystal structure of sodium ferrous sulfate determines that it has inherent defects as a positive electrode material for sodium ion batteries. For example, there are certain problems with the deintercalation of sodium in sodium ferrous sulfate, resulting in its low capacity. How to deintercalate as many sodium ions as possible has become one of the keys to preparing this high-performance material. At the same time, the dissolution of iron is also an important indicator that affects the performance of sodium ferrous sulfate. How to avoid the dissolution of iron is also the key to preparing sodium ferrous sulfate materials.

[0003] Sodium ferroaluminate is a light yellow crystal with coarse particles, fast precipitation speed and easy filtering. Sodium ferroaluminate exists in the iron removal slag of hydrometallurgy and is generally discharged as the iron removal slag. At the same time, the preparation method of sodium ferroaluminate is simple and the preparation cost is low. The conventional preparation method of sodium ferroaluminate is: sodium sulfate is added to ferric sulfate in an aqueous solution, and reacted at high temperature and high pH to obtain sodium ferroaluminate. The specific reaction equation is as follows: 3Fe 2 (SO 4 ) 3 +12H 2 O+Na 2 SO 4 =Na 2 Fe 6 (SO 4 ) 4 (OH) 12 +6H 2 SO 4 . At present, one of the synthetic routes for preparing sodium ferrous sulfate positive electrode materials using sodium ferrous alum is: using sulfuric acid to decompose sodium ferrous alum to obtain iron sulfate and sodium sulfate, and then adding sodium sulfate and coating carbon to form a sodium ferrous sulfate positive electrode material. However, the above route is relatively cumbersome and requires the sodium ferrous alum to be decomposed in advance. The second synthetic route for preparing sodium ferrous sulfate positive electrode materials using sodium ferrous alum is: mixing sodium ferrous alum, sodium sulfate, phosphoric acid, ammonium bicarbonate, and a carbon source into a ball-milled slurry, and spray-dried and calcined to obtain a sodium ferrous sulfate positive electrode material. The above process requires decomposition and high-temperature calcination, has a long process flow, and the sodium ferrous sulfate positive electrode material prepared has a low sodium content.

[0004] Therefore, it is urgent to propose a new synthesis route for preparing sodium ferrous sulfate positive electrode material using yellow sodium ferrous alum to solve the shortcomings of the existing synthesis process. Summary of the invention

[0005] In view of the technical problems existing in the background technology, the present application provides a basic sodium ferrous sulfate positive electrode material and a preparation method and application thereof, aiming to solve the technical problems in the prior art of using yellow sodium ferrous sulfate to prepare the sodium ferrous sulfate positive electrode material, which has a cumbersome synthesis route, high energy consumption, and low sodium content in the prepared sodium ferrous sulfate positive electrode material.

[0006] In the first aspect, the present invention provides a basic sodium ferrous sulfate positive electrode material, the basic sodium ferrous sulfate positive electrode material has the structural formula: Na 8 Fe 6 (SO 4 ) 4 (OH) 12 The compaction density of the basic sodium ferrous sulfate positive electrode material is 2.2-2.3 g / mL, and the BET specific surface area is 3-6 m 2 / g, powder resistivity is greater than 60Ω.cm.

[0007] In the technical solution of the embodiment of the present application, the structural formula of the sodium ferrous sulfate positive electrode material is Na 8 Fe 6 (SO 4 ) 4 (OH) 12 It contains 8 sodium ions, of which 5-6 can be effectively released. It has a higher specific capacity, a higher compaction density, and a relatively high voltage. At the same time, its BET is relatively low, and the trivalent iron content and iron dissolution are relatively low.

[0008] In a second aspect, the present application provides a method for preparing a basic sodium ferrous sulfate positive electrode material, comprising the following steps: Mixing natrona, sodium sulfite, urea and water to obtain a first mixed slurry; The first mixed slurry is subjected to a hydrothermal reaction to obtain a reaction slurry, and then the reaction slurry is filtered, washed and dried to obtain a basic sodium ferrous sulfate positive electrode material.

[0009] In the technical scheme of the embodiment of the present application, with cheap yellow sodium iron alum as the matrix, under the hydrothermal environment of high temperature and high pressure, in the presence of sodium sulfite, ferric iron is reduced to ferrous iron, and the sodium therein is compounded to the matrix, thereby obtaining a basic sodium ferrous sulfate positive electrode material; the present application also introduces urea, urea decomposes at high temperature, and the ammonia produced is dissolved in water, while consuming a large amount of hydrogen ions produced, thereby effectively stabilizing the pH of the solution, avoiding the low purity of the product caused by too large pH fluctuations. In addition, under the hydrothermal environment of high temperature and high pressure, the crystallinity of the obtained product is also higher. The present invention avoids the traditional sintering process and directly adopts the high temperature hydrothermal method for preparation. The process energy consumption of the present invention is lower, the process route is shorter, and the sodium content, capacity and compaction density of the basic sodium ferrous sulfate positive electrode material prepared by the present invention are higher.

[0010] In some embodiments, the particle size D50 of natarosite is 3-10 μm; the molar ratio of natarosite to sodium sulfite is 1:(3.5-4); the molar ratio of natarosite to urea is 1:(3-4); and the solid content of the first mixed slurry is 25%-35%.

[0011] In this embodiment, by controlling the particle size of sodium ferroaluminate within the range, it is conducive to sufficient reaction and high particle dispersibility. If the particle size of sodium ferroaluminate is low, strong agglomeration may occur during the reaction, resulting in unevenness between particles; if the particle size of sodium ferroaluminate is high, the final reaction may be insufficient, and sodium and sulfate cannot fully penetrate into the material. By controlling the molar ratio of sodium ferroaluminate to sodium sulfite within the above range, the reaction can be more sufficient and avoid wasting sodium sulfite, and basic sodium ferrous sulfate can be effectively formed to form a sodium-rich structure. By controlling the molar ratio of sodium ferroaluminate to urea within the above range, basic sodium ferrous sulfate can be effectively synthesized; if the amount of urea added is too high, the pH in the solution is too high, and a large amount of hydroxide will be generated; if the amount of urea added is too low, the concentration of hydroxide will be too low, making it difficult to generate basic ferrous sulfate. By controlling the solid content of the first mixed slurry within the range, the hydrothermal reaction can proceed smoothly, agglomeration between particles can be avoided, dispersibility is better, and production efficiency is improved.

[0012] In some embodiments, the first mixed slurry also includes: a dispersant; and the dispersant is polyethylene glycol; the amount of the dispersant added is 0.1%-0.5% of the water mass; during the hydrothermal reaction, the reaction temperature is 170-250°C, the reaction pressure is 8-15kg, the reaction time is 8-15h, and the hydrothermal reaction is carried out under stirring conditions, and the stirring speed is 100-300r / min.

[0013] In this embodiment, by adding a dispersant, not only can the uniform dispersion of the system be achieved, agglomeration between particles is avoided, and uniform suspension between particles is achieved, and the primary particle size is more uniform, but also a matrix and foundation can be provided for the carbon coating process that may exist later, so that the carbon coating layer is more uniform. By controlling the temperature, pressure, and time of the hydrothermal reaction within this range, basic sodium ferrous sulfate can be obtained by reaction. If the reaction temperature is too high, the pressure is too high, or the time is too long, the primary particles of the material will be too large, thereby affecting the electrical properties; if the reaction temperature is too low, the pressure is too low, or the time is too short, the crystallinity of the material will be too low, so that the iron dissolution is high and the cycle performance is reduced.

[0014] In some embodiments, drying includes a first drying and a second drying, the first drying is spray drying, and the second drying is vacuum drying or drying under protective gas; wherein, the inlet air temperature of spray drying is 150-250°C, the outlet air temperature of spray drying is 80-90°C, the spray particle size D50 of spray drying is 3-15μm, and the water content of the basic sodium ferrous sulfate positive electrode material obtained by spray drying is ≤0.3%; the drying temperature of vacuum drying is 100-130°C, and the water content of the basic sodium ferrous sulfate positive electrode material obtained by vacuum drying is ≤400ppm; the drying temperature of drying under protective gas is 100-130°C, and the water content of the basic sodium ferrous sulfate positive electrode material obtained by drying under protective gas is ≤400ppm; the protective gas is nitrogen or argon.

[0015] In this embodiment, spherical particles are formed by spray drying, which can avoid agglomeration during the homogenization process, thereby effectively improving the processing performance of the material. At the same time, the morphology of the spherical particles can effectively avoid the absorption of water, thereby effectively reducing the moisture content of the material. In addition, the carbon material (if added) can be coated on the surface of the basic sodium ferrous sulfate; by vacuum drying or drying under protective gas, the moisture in the spray-dried material can be further removed.

[0016] In a third aspect, the present invention provides a carbon-coated sodium ferrous sulfate positive electrode material, the structural formula of the carbon-coated sodium ferrous sulfate positive electrode material is: Na 8 Fe 6 (SO 4 ) 4 (OH) 12 @C; The compaction density of the carbon-coated sodium ferrous sulfate cathode material is 2.2-2.3 g / mL, and the BET specific surface area is 3-6 m 2 / g, powder resistivity is 10-60 Ω.cm.

[0017] In the technical solution of the embodiment of the present application, the basic sodium ferrous sulfate positive electrode material has a lower powder resistivity after being carbon-coated, which can improve the conductivity of the battery.

[0018] In a fourth aspect, an embodiment of the present application provides a method for preparing a carbon-coated basic sodium ferrous sulfate positive electrode material, comprising the following steps: Mixing natrona, sodium sulfite, urea and water to obtain a first mixed slurry; The first mixed slurry is subjected to a hydrothermal reaction, and then filtered and washed to obtain a washed material; Mixing the washing material, the antioxidant, the carbon material and water to obtain a second mixed slurry; Grinding the second mixed slurry to obtain a ground slurry; The ground slurry is dried to obtain a carbon-coated basic sodium ferrous sulfate positive electrode material.

[0019] In this embodiment, by adding an antioxidant, ferrous ions can be prevented from being oxidized during reactions and other processes; by adding carbon materials, carbon coating of the sodium ferrous sulfate basic cathode material can be achieved, thereby improving the conductivity of the cathode material; through mixed grinding, the material can be made more dispersed and is conducive to carbon coating and deposition, so that the powder resistivity of the material is lower, the electronic conductivity is better, and the capacity is better.

[0020] In some embodiments, the antioxidant is hydrazine hydrate; the amount of the antioxidant added is 0.2%-0.5% of the mass of the second mixed slurry; the carbon material is an inorganic carbon material; the amount of the carbon material added is 0.01%-5% of the mass of the solid content in the washing material; the solid content of the second mixed slurry is 10-50wt%; the particle size D50 of the grinding slurry is 300-400nm.

[0021] In this embodiment, by selecting hydrazine hydrate as an antioxidant, it can be decomposed into gas at high temperature without residue. If the amount of antioxidant added is too high, it will cause waste, and if the amount of antioxidant added is too low, it will not have an antioxidant effect. If the amount of carbon material added is too much, the proportion of inactive substances is increased, which will reduce the energy density of the battery; if the amount of carbon material added is too little, the positive electrode material may be directly exposed to the electrolyte, resulting in the occurrence of side reactions and reducing the capacity. At the same time, the positive electrode material may undergo structural changes or pulverization during the cycle, resulting in a decrease in cycle performance.

[0022] In a fifth aspect, an embodiment of the present application provides a positive electrode plate, comprising the basic sodium ferrous sulfate positive electrode material provided in the first aspect of the present application or the carbon-coated basic sodium ferrous sulfate positive electrode material provided in the third aspect.

[0023] In the technical solution of the embodiment of the present application, the positive electrode plate includes the above-mentioned basic sodium ferrous sulfate positive electrode material or the carbon-coated basic sodium ferrous sulfate positive electrode material, and thus has the advantages of high specific capacity, high compaction density and relatively high voltage.

[0024] In a sixth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate provided in the fifth aspect of the present application.

[0025] In the technical solution of the embodiment of the present application, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantages of high specific capacity, high compaction density and relatively high voltage.

[0026] Compared with the prior art, the beneficial effects of this application include: The basic sodium ferrous sulfate positive electrode material of the present application has a higher sodium content, a higher capacity, a higher compaction density, a relatively high voltage, excellent performance, and a simple preparation method, and is suitable for industrial promotion.

[0027] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 A process flow chart of an embodiment of a method for preparing a basic sodium ferrous sulfate positive electrode material provided in an embodiment of the present application; Figure 2 This is a SEM image of the sodium ferroalloy used in Example 1 of the present application; Figure 3 This is a SEM image of the graphene-coated sodium ferrous sulfate positive electrode material obtained in Example 1 of the present application; Figure 4 0.2C and 1C charge-discharge curves of the graphene-coated sodium ferrous sulfate positive electrode material obtained in Example 1 of the present application. DETAILED DESCRIPTION

[0030] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0032] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0033] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0034] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0035] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0036] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0037] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0038] At present, one of the synthetic routes for preparing sodium ferrous sulfate positive electrode materials using natrona is: using sulfuric acid to decompose natrona to obtain iron sulfate and sodium sulfate, then adding sodium sulfate and coating carbon to form sodium ferrous sulfate positive electrode materials. However, the above route is relatively cumbersome and requires the natrona to be decomposed in advance. The second synthetic route for preparing sodium ferrous sulfate positive electrode materials using natrona is: mixing natrona, sodium sulfate, phosphoric acid, ammonium bicarbonate, and a carbon source into a ball-milled slurry, spray-dried, and calcined to obtain a sodium ferrous sulfate positive electrode material. However, the above routes all use a calcination process, which has a long process flow, high energy consumption, and low sodium content.

[0039] In order to solve the technical problems of complicated synthesis route, high energy consumption and low sodium content in the preparation of sodium ferrous sulfate positive electrode materials using yellow sodium ferroaluminate in the prior art, the present application provides a basic sodium ferrous sulfate positive electrode material and its preparation method and application. Among them, the present application uses yellow sodium ferroaluminate crystals as raw materials, and obtains a high-performance basic sodium ferrous sulfate positive electrode material through a reduction reaction under high temperature and high pressure. The material has higher sodium content, higher capacity, higher compaction density, and relatively high voltage, excellent performance, and a simple preparation method, which is suitable for industrial promotion, thereby improving the performance of positive electrode sheets and secondary batteries.

[0040] In the first aspect, the present invention provides a basic sodium ferrous sulfate positive electrode material, the basic sodium ferrous sulfate positive electrode material has the structural formula: Na 8 Fe 6 (SO 4 ) 4 (OH) 12 ; Its compacted density is 2.2-2.3 g / mL, including but not limited to 2.2 g / mL, 2.22 g / mL, 2.24 g / mL, 2.26 g / mL, 2.28 g / mL, 2.3 g / mL; BET specific surface area is 3-6 m 2 / g, including but not limited to 3m 2 / g, 3.5m 2 / g, 4m 2 / g, 4.5m 2 / g, 5m 2 / g, 5.5m2 / g, 6m 2 / g, etc.; powder resistivity is greater than 60Ω.cm.

[0041] In the technical solution of the embodiment of the present application, the basic sodium ferrous sulfate positive electrode material contains 8 sodium ions, of which 5-6 sodium ions can be effectively released, and its specific capacity is higher, the compaction density is higher, and the voltage is also relatively high. At the same time, its BET is relatively low, and the trivalent iron content and iron dissolution are relatively low.

[0042] Please refer to Figure 1 In a second aspect, the present application provides a method for preparing a basic sodium ferrous sulfate positive electrode material, comprising the following steps: S1, mixing yellow sodium ferroalloy, sodium sulfite, urea and water to obtain a first mixed slurry; S2. The first mixed slurry is subjected to a hydrothermal reaction to obtain a reaction slurry. Thereafter, the reaction slurry is filtered, washed and dried to obtain a basic sodium ferrous sulfate positive electrode material.

[0043] In the technical scheme of the embodiment of the present application, with cheap yellow sodium iron alum as the matrix, under the hydrothermal environment of high temperature and high pressure, in the presence of sodium sulfite, the trivalent iron is reduced to divalent iron, and the sodium therein is compounded to the matrix, thereby obtaining a basic sodium ferrous sulfate positive electrode material; the present application also introduces urea, which decomposes at high temperature, and the ammonia produced is dissolved in water, while consuming a large amount of hydrogen ions produced, thereby effectively stabilizing the pH of the solution, avoiding the low purity of the product caused by too large pH fluctuations. In addition, under the hydrothermal environment of high temperature and high pressure, the crystallinity of the obtained product is also higher. The present invention avoids the traditional sintering process and directly adopts the high temperature hydrothermal method for preparation. The process energy consumption of the present invention is lower, the process route is shorter, and the sodium content and compaction density of the basic sodium ferrous sulfate positive electrode material prepared by the present invention are higher.

[0044] During the hydrothermal reaction, the chemical reaction equation is as follows: Na 2 Fe 6 (SO 4 ) 4 (OH) 12 +3Na 2 SO 3 +3H 2 O=Na 8 Fe 6 (SO 4 ) 4 (OH) 12 +3H 2 SO 4 CO(NH 2 ) 2+ 3H 2 O = CO 2 ↑ + 2NH 3 .H 2 O 2NH 3 +H 2 SO 4 =(NH 4 ) 2 SO 4 Further, in some embodiments, in step S1, the particle size D50 of sodium ferroaluminate is 3-10 μm, including but not limited to 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc., which is not limited in the present application.

[0045] In the technical solution of the embodiment of the present application, by controlling the particle size of sodium ferroalcite within this range, it is conducive to sufficient reaction and high particle dispersion. If the particle size of sodium ferroalcite is too small, strong agglomeration may occur during the reaction, resulting in unevenness between particles; if the particle size of sodium ferroalcite is too high, the final reaction may be insufficient, and sodium and sulfate cannot fully penetrate into the material.

[0046] Furthermore, in some embodiments, the particle size D50 of natto iron alum is ground to 3-10 μm by ball milling.

[0047] Further, in some embodiments, in step S1, the molar ratio of natantia ferrocyanide to sodium sulfite is 1:(3.5-4), including but not limited to 1:3.5, 1:3.6, 1:3.7, 1:3.8, 1:3.9, 1:4, etc., which is not limited in the present application.

[0048] In the technical solution of the embodiment of the present application, by controlling the molar ratio of natanoic acid alum to sodium sulfite within the above range, the reaction can be made more complete and the waste of sodium sulfite can be avoided. At the same time, basic sodium ferrous sulfate can be effectively formed to form a sodium-rich structure.

[0049] Further, in some embodiments, in step S1, the molar ratio of sodium ferroaluminate to urea is 1:(3-4), including but not limited to 1:3, 1:3.2, 1:3.4, 1:3.6, 1:3.8, 1:4, etc., which is not limited in the present application.

[0050] In the technical solution of the embodiment of the present application, by controlling the molar ratio of sodium ferrous sulfate to urea within the above range, basic sodium ferrous sulfate can be effectively synthesized; if the amount of urea added is too high, the pH of the solution will be too high, resulting in the presence of a large amount of ferrous hydroxide, making the hydroxide content too high; if the amount of urea added is too low, the hydroxide concentration will be too low, making it difficult to generate basic ferrous sulfate.

[0051] Further, in some embodiments, in step S1, the solid content of the first mixed slurry is 25%-35%, including but not limited to 25%, 27%, 29%, 31%, 33%, 35%, etc., which is not limited in the present application.

[0052] In the technical solution of the embodiment of the present application, by controlling the solid content of the first mixed slurry within this range, the hydrothermal reaction can proceed smoothly, agglomeration between particles can be avoided, dispersibility is better, and production efficiency is improved.

[0053] Furthermore, in some embodiments, in step S1, the first mixed slurry further includes: a dispersant.

[0054] In the technical solution of the embodiment of the present application, by adding a dispersant, not only can the system be uniformly dispersed, agglomeration between particles can be avoided, the particles can be evenly suspended, and the primary particle size can be more uniform, but it can also provide a matrix and foundation for the subsequent possible carbon coating process, making the carbon coating layer more uniform.

[0055] The present application does not limit the type of dispersant, and those skilled in the art can select according to actual conditions. In some specific embodiments, the dispersant is polyethylene glycol, including but not limited to polyethylene glycol 1000, polyethylene glycol 2000, polyethylene glycol 3000, etc.

[0056] Furthermore, in some embodiments, the amount of dispersant added is 0.1%-0.5% of the water mass, including but not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, etc., which is not limited in this application.

[0057] Further, in some embodiments, in step S2, during the hydrothermal reaction, the reaction temperature is 170-250°C, including but not limited to 170°C, 190°C, 210°C, 230°C, 250°C, etc., and the present application does not limit this; the reaction pressure is 8-15kg, including but not limited to 8kg, 9kg, 10kg, 11kg, 12kg, 13kg, 14kg, 15kg, etc., and the present application does not limit this; the reaction time is 8-15h, including but not limited to 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, etc., and the present application does not limit this. It should be noted that 1kg pressure is equivalent to 0.1MPa.

[0058] In the technical solution of the embodiment of the present application, by controlling the temperature, pressure and time of the hydrothermal reaction within this range, basic sodium ferrous sulfate can be obtained by reaction. If the reaction temperature is too high, the pressure is too high or the time is too long, the primary particles will be too large, so that the migration distance of sodium is too far, affecting the capacity; if the reaction temperature is too low, the pressure is too low or the time is too short, the crystallinity will be incomplete, so that the iron dissolution is too high, affecting the cycle performance.

[0059] Furthermore, in some embodiments, in step S2, during the hydrothermal reaction, the reaction is carried out under stirring conditions.

[0060] Furthermore, in some embodiments, the stirring speed is 100-300 r / min, including but not limited to 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, etc., which is not limited in the present application.

[0061] Furthermore, in some embodiments, in step S2, during the washing process, washing with pure water is stopped after washing until the conductivity is ≤100 μS / cm.

[0062] Further, in some embodiments, in step S2, drying includes first drying and second drying, the first drying is spray drying, and the second drying is vacuum drying or drying under protective gas.

[0063] In the technical solution of the embodiment of the present application, spherical particles are formed by spray drying, which can avoid agglomeration in the homogenization process, thereby effectively improving the processing performance of the material. At the same time, the morphology of the spherical particles can effectively avoid the absorption of water, thereby effectively reducing the moisture content of the material. In addition, the carbon material (if added) can be coated on the surface of sodium ferrous sulfate. By vacuum drying or drying under protective gas, the moisture in the spray-dried material can be further removed.

[0064] Furthermore, in some embodiments, the inlet air temperature of spray drying is 150-250°C, including but not limited to 150°C, 170°C, 190°C, 210°C, 230°C, 250°C, etc., which is not limited in the present application; the outlet air temperature of spray drying is 80-90°C, including but not limited to 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, etc., which is not limited in the present application.

[0065] Furthermore, in some embodiments, the spray particle size D50 of spray drying is 3-15μm, including but not limited to 3μm, 5μm, 7μm, 9μm, 11μm, 13μm, 15μm, etc., which is not limited in the present application; the water content of the basic sodium ferrous sulfate positive electrode material obtained by spray drying is ≤0.3%.

[0066] Further, in some specific embodiments, the drying temperature of vacuum drying is 100-130°C, including but not limited to 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, etc., which is not limited in the present application; the water content of the sodium ferrous sulfate positive electrode material obtained by vacuum drying is ≤400ppm.

[0067] Further, in some specific embodiments, the drying temperature under protective gas is 100-130°C, including but not limited to 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, etc., and the present application is not limited to this; the water content of the basic sodium ferrous sulfate positive electrode material obtained by drying under protective gas is ≤400ppm; the protective gas includes but is not limited to nitrogen or argon, etc.

[0068] Furthermore, in some embodiments, in step S2, after drying, the process further includes: cooling the dried material, taking it out, screening, removing iron and packaging to obtain basic sodium ferrous sulfate positive electrode material.

[0069] In the technical solution of the embodiment of the present application, large particles can be effectively avoided by screening, removing iron and packaging the dry materials, so that the pole pieces are flat during the coating process, while the magnetic substances are reduced and the moisture content of the product is controlled.

[0070] Furthermore, in some specific embodiments, the screening process uses a 100-200 mesh ultrasonic vibration screen.

[0071] Furthermore, in some specific embodiments, the packaging method is vacuum packaging; the packaging is carried out in a constant temperature and humidity room, the temperature is controlled at 25±5°C, and the humidity is ≤10%.

[0072] In a third aspect, the present application provides a carbon-coated sodium ferrous sulfate basic cathode material, the structural formula of the carbon-coated sodium ferrous sulfate basic cathode material is: Na 8 Fe 6 (SO 4 ) 4 (OH) 12 @C; its compacted density is 2.2-2.3g / mL, including but not limited to 2.2g / mL, 2.22g / mL, 2.24g / mL, 2.26g / mL, 2.28g / mL, 2.3g / mL; BET specific surface area is 3-6m 2 / g, including but not limited to 3m 2 / g, 3.5m 2 / g, 4m 2 / g, 4.5m 2 / g, 5m 2 / g, 5.5m 2 / g, 6m 2 / g, etc.; the trivalent iron content is 50-150ppm, including but not limited to 50ppm, 60ppm, 70ppm, 80ppm, 90ppm, 100ppm, 110ppm, 120ppm, 130ppm, 140ppm, 150ppm, etc.; the iron dissolution is 50-150ppm, including but not limited to 50ppm, 60ppm, 70ppm, 80ppm, 90ppm, 100ppm, 110ppm, 120ppm, 130ppm, 140ppm, 150ppm, etc.; the powder resistivity is 10-60Ω.cm, including but not limited to 10Ω.cm, 20Ω.cm, 30Ω.cm, 40Ω.cm, 50Ω.cm, 60Ω.cm, etc.

[0073] In the technical solution of the embodiment of the present application, the basic sodium ferrous sulfate positive electrode material has a lower powder resistivity after being carbon-coated, which can improve the conductivity of the battery.

[0074] In a fourth aspect, an embodiment of the present application provides a method for preparing a carbon-coated basic sodium ferrous sulfate positive electrode material, comprising the following steps: S10, mixing natronasite, sodium sulfite, urea and water to obtain a first mixed slurry; S20, subjecting the first mixed slurry to a hydrothermal reaction, and then filtering and washing to obtain a washed material; S30, mixing the washing material, the antioxidant, the carbon material and water to obtain a second mixed slurry; S40, grinding the second mixed slurry to obtain a grinding slurry; S50, drying the ground slurry to obtain a carbon-coated basic sodium ferrous sulfate positive electrode material.

[0075] In the technical solution of the embodiment of the present application, by adding an antioxidant, ferrous ions can be prevented from being oxidized during reactions and other processes; by adding carbon materials, carbon coating of the basic sodium ferrous sulfate positive electrode material can be achieved, thereby improving the conductivity of the positive electrode material; through mixed grinding, the material can be made more dispersed and conducive to carbon coating and deposition, so that the powder resistivity of the material is lower, the electronic conductivity is better, and the capacity is better.

[0076] In the present application, it should be noted that in the method for preparing the carbon-coated basic sodium ferrous sulfate positive electrode material, the raw material dosage, reaction conditions, etc. involved in step S10 and step S20 are consistent with the aforementioned method for preparing the basic sodium ferrous sulfate positive electrode material.

[0077] Further, in some embodiments, in step S30, the antioxidant is hydrazine hydrate.

[0078] In the technical solution of the embodiment of the present application, by selecting hydrazine hydrate as an antioxidant, it can be decomposed into gas at high temperature without residue.

[0079] Further, in some embodiments, in step S30, the amount of antioxidant added is 0.2%-0.5% of the mass of the second mixed slurry, including but not limited to 0.2%, 0.3%, 0.4%, 0.5%, etc., which is not limited in the present application.

[0080] In the technical solution of the embodiment of the present application, if the amount of antioxidant added is too high, it will cause waste, and if the amount of antioxidant added is too low, it will not play an antioxidant role.

[0081] Further, in some embodiments, in step S30, the carbon material is an inorganic carbon material. The present application does not limit the type of inorganic carbon material, and those skilled in the art can select it according to actual conditions. Further, in some specific embodiments, the inorganic carbon material is at least one of graphene, carbon nanotubes, carbon fibers, conductive carbon black, and nano-conductive graphite.

[0082] Further, in some embodiments, in step S30, the amount of carbon material added is 0.01%-5% of the mass of the solid content in the washing material, including but not limited to 0.01, 1%, 2%, 3%, 4%, 5%, etc., and the present application does not impose any limitation on this.

[0083] In the technical solution of the embodiment of the present application, if the amount of carbon material added is too much, the proportion of inactive substances increases, which will reduce the energy density of the battery; if the amount of carbon material added is too little, the positive electrode material may be directly exposed to the electrolyte, resulting in side reactions and reduced capacity. At the same time, the positive electrode material may undergo structural changes or pulverization during the cycle, resulting in a decrease in cycle performance.

[0084] Further, in some embodiments, in step S30, the carbon material is added in the form of an aqueous dispersion, and the mass fraction of the carbon material is 3%-10%, including but not limited to 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., which is not limited in this application.

[0085] Further, in some embodiments, in step S30, the solid content of the second mixed slurry is 10-50wt%, including but not limited to 10%, 20%, 30%, 40%, 50%, etc., which is not limited in the present application.

[0086] Further, in some embodiments, in step S40, the particle size D50 of the polishing slurry is 300-400 nm, including but not limited to 300 nm, 320 nm, 340 nm, 360 nm, 380 nm, 400 nm, etc., which is not limited in the present application.

[0087] Further, in some embodiments, in step S40, grinding is performed by a sand mill.

[0088] In the technical solution of the embodiment of the present application, grinding with a sand mill can make the material particle size finer and the dispersion better, which is beneficial to the uniformity of subsequent carbon coating.

[0089] Further, in some embodiments, in step S50, drying includes first drying and second drying, the first drying is spray drying, and the second drying is vacuum drying or drying under protective gas.

[0090] In the technical solution of the embodiment of the present application, spherical particles are formed by spray drying, which can avoid agglomeration in the homogenization process, thereby effectively improving the processing performance of the material. At the same time, the morphology of the spherical particles can effectively avoid the absorption of water, thereby effectively reducing the moisture content of the material. In addition, the carbon material can be coated on the surface of sodium ferrous sulfate. By vacuum drying or drying under protective gas, the moisture in the spray-dried material can be further removed.

[0091] Furthermore, in some embodiments, the inlet air temperature of spray drying is 150-250°C, including but not limited to 150°C, 170°C, 190°C, 210°C, 230°C, 250°C, etc., which is not limited in the present application; the outlet air temperature of spray drying is 80-90°C, including but not limited to 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, etc., which is not limited in the present application.

[0092] Furthermore, in some embodiments, the spray particle size D50 of spray drying is 3-15μm, including but not limited to 3μm, 5μm, 7μm, 9μm, 11μm, 13μm, 15μm, etc., which is not limited in the present application; the water content of the carbon-coated sodium ferrous sulfate positive electrode material obtained by spray drying is ≤0.3%.

[0093] Further, in some specific embodiments, the drying temperature of vacuum drying is 100-130°C, including but not limited to 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, etc., and the present application is not limited to this; the water content of the carbon-coated sodium ferrous sulfate positive electrode material obtained by vacuum drying is ≤400ppm.

[0094] Further, in some specific embodiments, the drying temperature under protective gas is 100-130°C, including but not limited to 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, etc., and the present application is not limited to this; the water content of the carbon-coated sodium ferrous sulfate positive electrode material obtained by drying under protective gas is ≤400ppm; the protective gas includes but is not limited to nitrogen or argon, etc.

[0095] Furthermore, in some embodiments, in step S50, after drying, the process further includes: cooling the dried material and taking it out, screening, removing iron and packaging to obtain a carbon-coated sodium ferrous sulfate positive electrode material.

[0096] In the technical solution of the embodiment of the present application, large particles can be effectively avoided by screening, removing iron and packaging the dry materials, so that the pole pieces are flat during the coating process, while the magnetic substances are reduced and the moisture content of the product is controlled.

[0097] Furthermore, in some specific embodiments, the screening process uses a 100-200 mesh ultrasonic vibration screen.

[0098] Furthermore, in some specific embodiments, the packaging method is vacuum packaging; the packaging is carried out in a constant temperature and humidity room, the temperature is controlled at 25±5°C, and the humidity is ≤10%.

[0099] In a fifth aspect, an embodiment of the present application provides a positive electrode plate, comprising the basic sodium ferrous sulfate positive electrode material provided in the first aspect of the present application or the carbon-coated basic sodium ferrous sulfate positive electrode material provided in the third aspect.

[0100] In the technical solution of the embodiment of the present application, the positive electrode plate includes the above-mentioned basic sodium ferrous sulfate positive electrode material or the carbon-coated basic sodium ferrous sulfate positive electrode material, and thus has the advantages of high specific capacity, high compaction density and relatively high voltage.

[0101] In a sixth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate provided in the fifth aspect of the present application.

[0102] In the technical solution of the embodiment of the present application, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantages of high specific capacity, high compaction density and relatively high voltage.

[0103] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.

[0104] 1. Preparation method Example 1 The sodium ferroalum is crushed to a material D50 of 8 μm, and then sodium sulfite, urea and pure water are added to slurry, and then polyethylene glycol 2000 is added to the slurried material to obtain a first mixed slurry; then, the mixture is reacted under high temperature and high pressure, with a stirring speed of 200 r / min, a temperature of 220°C, and a pressure of 12.5 kg for 12 hours to obtain a reactant; wherein the molar ratio of sodium ferroalum, sodium sulfite and urea is 1:3.8:3.5, and the solid content of the slurried material is 30%; the amount of polyethylene glycol 2000 added is 0.3% of the mass of pure water.

[0105] The reactant is filtered and washed with pure water until the conductivity is ≤100 μS / cm, and then the washing is stopped to obtain a basic sodium ferrous sulfate positive electrode material. Graphene slurry, hydrazine hydrate solution and pure water are added to the basic sodium ferrous sulfate positive electrode material to obtain a second mixed slurry, and the slurry is ground with a sand mill until the particle size D50 of the slurry is 345 nm, and then spray-dried. The spray-dried material is placed in a vacuum oven and dried until the moisture content of the material is ≤400 ppm, and then the drying is stopped. After cooling, it is taken out, and then sieved and iron removed with a 150-mesh ultrasonic vibration screen, and finally vacuum-packed in a constant temperature and humidity room to obtain a carbon-coated basic sodium ferrous sulfate positive electrode material; wherein, the solid content of the graphene slurry is 6%, and the mass of the graphene is 3% of the dry mass of the basic sodium ferrous sulfate positive electrode material; the concentration of the hydrazine hydrate solution is 12wt%, the mass of the hydrazine hydrate is 0.35% of the total mass of the second mixed slurry, and the solid content of the second mixed slurry is 25wt%; during the spray drying process, the inlet air temperature is 205℃, the outlet air temperature is 85℃, the spray particle size D50 is 7.1μm, and the moisture content is ≤0.3%; during the vacuum drying process, the drying temperature is 108℃; in the constant temperature and humidity room, the temperature is controlled at 25±5℃, and the humidity is ≤10%.

[0106] Example 2 The sodium ferroalum is crushed to a material D50 of 3 μm, and then sodium sulfite, urea and pure water are added to slurry, and then polyethylene glycol 2000 is added to the slurried material to obtain a first mixed slurry; then, the mixture is reacted under high temperature and high pressure, with a stirring speed of 100 r / min, a temperature of 170°C, and a pressure of 8 kg for 15 hours to obtain a reactant; wherein the molar ratio of sodium ferroalum, sodium sulfite and urea is 1:3.5:3, and the solid content of the slurried material is 25%; the amount of polyethylene glycol 2000 added is 0.1% of the mass of pure water.

[0107] After filtering the reactant, washing with pure water until the conductivity is ≤100 μS / cm, then stopping washing to obtain basic sodium ferrous sulfate positive electrode material, then adding graphene slurry, hydrazine hydrate solution and pure water to the basic sodium ferrous sulfate positive electrode material to obtain a second mixed slurry, and grinding it with a sand mill until the particle size D50 of the slurry is 300 nm, then spray drying, putting the spray-dried material into an oven, drying it under nitrogen gas protection until the material moisture is ≤400 ppm, then stopping drying, cooling and taking it out, and then sieving and removing iron with a 100-mesh ultrasonic vibration screen, and finally vacuum packaging in a constant temperature and humidity room to obtain a carbon coating Basic sodium ferrous sulfate positive electrode material; wherein, the solid content of the graphene slurry is 10%, and the mass of the graphene is 2% of the dry mass of the basic sodium ferrous sulfate positive electrode material; the concentration of the hydrazine hydrate solution is 12wt%, the mass of the hydrazine hydrate is 0.2% of the mass of the second mixed slurry, and the solid content of the second mixed slurry is 10wt%; during the spray drying process, the inlet air temperature is 150°C, the outlet air temperature is 80°C, the spray particle size D50 is 3μm, and the moisture content is ≤0.3%; during the drying process under nitrogen gas protection, the drying temperature is 100°C; in the constant temperature and humidity room, the temperature is controlled at 25±5°C, and the humidity is ≤10%.

[0108] Example 3 The sodium ferroaluminate is crushed to a material D50 of 10 μm, and then sodium sulfite, urea and pure water are added to slurry, and then polyethylene glycol 2000 is added to the slurried material to obtain a first mixed slurry; then, the mixture is reacted under high temperature and high pressure, with a stirring speed of 300 r / min, a temperature of 250°C, and a stirring reaction of 8 hours at a pressure of 15 kg to obtain a reactant; wherein the molar ratio of sodium ferroaluminate, sodium sulfite and urea is 1:4:4, and the solid content of the slurried material is 35%; the amount of polyethylene glycol 2000 added is 0.5% of the mass of pure water.

[0109] The reactant is filtered and washed with pure water until the conductivity is ≤100 μS / cm, and then the washing is stopped to obtain a basic sodium ferrous sulfate positive electrode material. Nano-conductive graphite slurry, hydrazine hydrate solution and pure water are added to the basic sodium ferrous sulfate positive electrode material to obtain a second mixed slurry, and the slurry is ground with a sand mill until the particle size D50 of the slurry is 400 nm, and then spray-dried. The spray-dried material is placed in a vacuum oven and dried until the moisture content of the material is ≤400 ppm, and then the drying is stopped. After cooling, it is taken out, and then sieved and iron removed with a 200-mesh ultrasonic vibration screen, and finally vacuum-packed in a constant temperature and humidity room to obtain a carbon-coated basic sodium ferrous sulfate positive electrode material; wherein, the solid content of the nano conductive graphite slurry is 3%, and the mass of the nano conductive graphite is 5% of the dry mass of the basic sodium ferrous sulfate positive electrode material; the concentration of the hydrazine hydrate solution is 12wt%, the mass of the hydrazine hydrate is 0.5% of the mass of the second mixed slurry, and the solid content of the second mixed slurry is 50wt%; during the spray drying process, the inlet air temperature is 250℃, the outlet air temperature is 90℃, the spray particle size D50 is 15μm, and the moisture content is ≤0.3%; during the vacuum drying process, the drying temperature is 130℃; in the constant temperature and humidity room, the temperature is controlled at 25±5℃, and the humidity is ≤10%.

[0110] Comparative Example 1 Compared with Example 2, the only difference is that the molar ratio of sodium ferroaluminate to urea is 1:2.5.

[0111] Comparative Example 2 Compared with Example 2, the only difference is that the molar ratio of sodium ferroaluminate to urea is 1:4.5.

[0112] Comparative Example 3 Compared with Example 2, the only difference is that the temperature of the hydrothermal reaction is 150°C.

[0113] Comparative Example 4 Compared with Example 2, the only difference is that the temperature of the hydrothermal reaction is 280°C.

[0114] 2. Test Method 1. Property test of yellow sodium ferrous sulfate, basic sodium ferrous sulfate positive electrode material and carbon-coated basic sodium ferrous sulfate positive electrode material 1. Na, Fe, S, Ca, Mg, Zn, Cu and Pb are detected by ICP; 2. C is tested by carbon-sulfur instrument; 3. D10, D50 and D90 are tested by laser particle size analyzer; 4. BET is determined by gas adsorption BET method; 5. The powder resistivity is tested by four-probe method with a test pressure of 10MPa; 6. PD (compacted density) test pressure is 3T; 7. pH and free sodium test: Take 10g of material, add 90g of water, stir for 15min at 25±1℃, then filter and test the pH and sodium content of the solution; 8. Iron dissolution test: Take 10g of material, add 90g of 0.05mol / L hydrochloric acid, stir for 15min at 25±1℃, then filter and test the iron content of the solution; 9. The moisture content is tested by KF moisture test method; 10. Ferric iron is measured by colorimetry.

[0115] 2. Properties test of secondary batteries The positive electrode material prepared in the embodiment was assembled into a button battery and its electrical performance was tested. The test process was as follows: 1. Reagents and Materials 1.1 Electrolyte: 1 mol / L sodium hexafluorophosphate (NaPF 6 ) and ethylene glycol dimethyl ether (DME) composed of sodium ion battery electrolyte; 1.2 N-methylpyrrolidone (battery grade); 1.3 Polyvinylidene fluoride (PVDF); 1.4 Acetylene black; 1.5 Aluminum foil with a thickness of 15 μm; 1.6 Metal sodium sheet with a thickness of 0.15 mm; 1.7 Polypropylene microporous diaphragm (for sodium batteries only).

[0116] 2. Preparation of positive electrode In the positive electrode slurry, the mass ratio of carbon-coated basic sodium ferrous sulfate positive electrode material to acetylene black (conductive agent) and polyvinylidene fluoride (binder) is 90:5:5, and the mass is accurate to 0.001g. Aluminum foil is used as the current collector for the positive electrode sheet. The carbon-coated basic sodium ferrous sulfate positive electrode material, acetylene black, PVDF and N-methylpyrrolidone are stirred and slurried, and the slurry is evenly coated on the aluminum foil, dried in an oven at 100°C, and cut into electrode sheets with a diameter of 15mm and a thickness of 0.1mm. The electrode sheets are weighed and the mass is accurate to 0.0001g. The mixing and coating process is strictly controlled, and the area and thickness of the electrode sheet to be tested must be consistent to avoid these factors affecting the test results.

[0117] 3. Battery Assembly In an inert gas glove box with water and oxygen content ≤ 0.0005%, a sodium metal sheet was used as the negative electrode material, a polypropylene microporous film was used as the separator, and 1 mol / L sodium hexafluorophosphate (NaPF 6) and ethylene glycol dimethyl ether (DME) as the sodium ion battery electrolyte, which were assembled into test cells. After the cells were sealed, they were tested using a sodium ion battery electrochemical performance tester.

[0118] 4. Battery Testing The prepared test battery was charged and discharged on a sodium ion battery electrochemical performance tester. The charge and discharge regime was as follows: (a) Under 25°C conditions, charging at a rate of 0.2C / 1C, the charging limit voltage is 4.5V; (b) Discharge at 25°C, 0.2C / 1C rate, and a discharge termination voltage of 2.0V; (c) Under -20℃ conditions, charge and discharge at a current rate of 1C, the charge limit voltage is 4.5V, and the discharge termination voltage is 2.0V.

[0119] III. Analysis of test results of various embodiments and comparative examples Table 1 Physical and chemical indicators of sodium ferroaluminate used in the examples and comparative examples

[0120] Table 2 Physical and chemical indicators of carbon-coated basic sodium ferrous sulfate positive electrode material obtained in Example 1

[0121] Table 3 Indicators of the carbon-coated basic sodium ferrous sulfate positive electrode material obtained in Example 2-3

[0122] Table 4 Indicators of the carbon-coated sodium ferrous sulfate positive electrode materials obtained in Comparative Examples 1-4

[0123] Please refer to Table 1. It can be seen from the data in Table 1 that the raw material yellow sodium ferroaluminate used in Example 1 has a small BET and a high tap density. Further, in this application, the compaction density of the prepared sodium ferrous sulfate positive electrode material is measured to be in the range of 2.2-2.3 g / mL, and the BET specific surface area is in the range of 3-6 m 2 / g, and the powder resistivity is relatively high.

[0124] Further, please refer to Table 2-3. It can be seen from the data in Table 2-3 that the BET of the product obtained in Example 1-3 is relatively low, the moisture content is low, the powder resistivity is low, and the trivalent iron content is also relatively low, but the compaction density is high and the capacity is also high. At the same time, the low-temperature performance of the material of the present application is excellent.

[0125] Further, please refer to Table 4. It can be seen from the data in Table 4 that a molar ratio of sodium ferroaluminate to urea that is too high or too low, or a temperature of the hydrothermal reaction that is too high or too low, will lead to a significant decrease in the capacity and cyclability of the sodium ferrous sulfate positive electrode material.

[0126] For further information, please refer to Figure 2 From the SEM results, the raw material yellow sodium ferroaluminate used in this Example 1 is spherical and granular.

[0127] For further information, please refer to Figure 3 From the SEM results, the product obtained in Example 1 is spherical particles with a primary particle size of about 150-250nm and a high degree of density. The compaction density of the product can reach more than 2.25g / mL. However, in the conventional sintering process, due to the decomposition of sulfate, the sintering temperature is not higher than 400°C, so the compaction density is generally lower, generally lower than 2.1g / mL.

[0128] For further information, please refer to Figure 4 From the charge and discharge curve, the capacity of the product obtained in Example 1 is relatively high, the charging capacity at 0.2C reaches more than 100mAh / g, the discharge capacity is 98mAh / g, and the discharge capacity at 1C is 92mAh / g. The electrical performance is excellent, and the median discharge voltage at 1C can reach about 3.8V, with a high voltage platform. In addition, the low-temperature performance of the material of the present invention is extremely excellent.

[0129] In summary, the process of the present invention has lower energy consumption and a shorter process route, and the basic sodium ferrous sulfate positive electrode material prepared by the present invention has higher sodium content, capacity and compaction density and excellent low-temperature performance.

[0130] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A sodium ferrous sulfate basic cathode material, characterized in that: The structural formula of the basic sodium ferrous sulfate positive electrode material is: Na8Fe6(SO4)4(OH) 12 ; The compaction density of the basic sodium ferrous sulfate positive electrode material is 2.2-2.3 g / mL, and the BET specific surface area is 3-6 m 2 / g, powder resistivity is greater than 60Ω.cm.

2. A method for preparing the basic sodium ferrous sulfate positive electrode material as claimed in claim 1, characterized in that: The following steps are involved: Mixing natrona, sodium sulfite, urea and water to obtain a first mixed slurry; The first mixed slurry is subjected to a hydrothermal reaction to obtain a reaction slurry, and then the reaction slurry is filtered, washed and dried to obtain a basic sodium ferrous sulfate positive electrode material.

3. The method for preparing the sodium ferrous sulfate positive electrode material according to claim 2, characterized in that: The particle size D50 of the soda ferroalite is 3-10 μm; the molar ratio of the soda ferroalite to sodium sulfite is 1:(3.5-4); the molar ratio of the soda ferroalite to urea is 1:(3-4); and the solid content of the first mixed slurry is 25%-35%.

4. The method for preparing the sodium ferrous sulfate positive electrode material according to claim 2, characterized in that: The first mixed slurry further includes: a dispersant; and / or The dispersant is polyethylene glycol; and / or The amount of the dispersant added is 0.1%-0.5% of the mass of the water; and / or During the hydrothermal reaction, the reaction temperature is 170-250° C., the reaction pressure is 8-15 kg, the reaction time is 8-15 h, and the hydrothermal reaction is carried out under stirring at a stirring speed of 100-300 r / min.

5. The method for preparing the sodium ferrous sulfate positive electrode material according to claim 2, characterized in that: The drying includes a first drying and a second drying, wherein the first drying is spray drying, and the second drying is vacuum drying or drying under protective gas; wherein, The inlet air temperature of the spray drying is 150-250°C, the outlet air temperature of the spray drying is 80-90°C, the spray particle size D50 of the spray drying is 3-15 μm, and the water content of the basic sodium ferrous sulfate positive electrode material obtained by the spray drying is ≤0.3%; and / or The drying temperature of the vacuum drying is 100-130° C., and the water content of the basic sodium ferrous sulfate positive electrode material obtained by the vacuum drying is ≤400ppm; and / or The drying temperature of the drying under the protective gas is 100-130° C., and the water content of the basic sodium ferrous sulfate positive electrode material obtained by drying under the protective gas is ≤400ppm; the protective gas is nitrogen or argon.

6. A carbon-coated basic sodium ferrous sulfate positive electrode material, characterized in that: The structural formula of the carbon-coated sodium ferrous sulfate cathode material is: Na8Fe6(SO4)4(OH) 12 @C; The carbon-coated basic sodium ferrous sulfate positive electrode material has a compaction density of 2.2-2.3 g / mL and a BET specific surface area of ​​3-6 m 2 / g, powder resistivity is 10-60 Ω.cm.

7. A method for preparing the carbon-coated basic sodium ferrous sulfate positive electrode material as claimed in claim 6, characterized in that: The following steps are involved: Mixing natrona, sodium sulfite, urea and water to obtain a first mixed slurry; The first mixed slurry is subjected to a hydrothermal reaction, and then filtered and washed to obtain a washed material; Mixing the washing material, antioxidant, carbon material and water to obtain a second mixed slurry; Grinding the second mixed slurry to obtain a ground slurry; The grinding slurry is dried to obtain a carbon-coated basic sodium ferrous sulfate positive electrode material.

8. The method for preparing the carbon-coated basic sodium ferrous sulfate positive electrode material according to claim 7, characterized in that: The antioxidant is hydrazine hydrate; and / or The amount of the antioxidant added is 0.2%-0.5% of the mass of the second mixed slurry; and / or The carbon material is an inorganic carbon material; and / or The amount of the carbon material added is 0.01%-5% of the solid content in the washing material; and / or The solid content of the second mixed slurry is 10-50wt%; and / or The particle size D50 of the grinding slurry is 300-400nm.

9. A positive electrode sheet, characterized in that: The positive electrode plate comprises the basic sodium ferrous sulfate positive electrode material according to claim 1 or the carbon-coated basic sodium ferrous sulfate positive electrode material according to claim 6.

10. A secondary battery, characterized in that: The secondary battery comprises the positive electrode sheet according to claim 9.