Method for producing positive electrode active material

By heat treatment and calcination in an atmospheric atmosphere, a lithium composite oxide with a layered rock salt structure is formed, which solves the high cost and low productivity problems caused by the use of oxygen atmosphere in the existing technology, and improves the output performance and performance of lithium-ion secondary batteries. capacity.

CN118724078APending Publication Date: 2024-10-01PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410365279.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology requires an oxygen atmosphere when manufacturing lithium composite oxides with high nickel content, resulting in high manufacturing costs and low productivity. In addition, high-temperature calcination inhibits the crystal growth of lithium composite oxides and affects battery output performance.

Method used

Heat treatment is performed in an atmospheric atmosphere to convert hydroxides with high nickel content into spinel structure oxides, which are mixed with lithium compounds and then calcined in an atmospheric atmosphere to form a lithium composite oxide with a layered rock salt structure, avoiding the use of oxygen. atmosphere, optimizing the peak integrated intensity ratio to improve the output characteristics of lithium-ion secondary batteries.

Benefits of technology

It is possible to manufacture cathode active materials with high nickel content without using an oxygen atmosphere, improve the output performance and capacity of lithium-ion secondary batteries, and reduce the manufacturing cost and complexity of the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724078A_ABST
    Figure CN118724078A_ABST
Patent Text Reader

Abstract

Provided is a method capable of producing a positive electrode active material that can impart a high output to a lithium ion secondary battery and has a high nickel content without using an oxygen atmosphere. A method for producing a positive electrode active material according to the present invention comprises: a step for obtaining an oxide having a spinel structure main body by heat-treating a hydroxide in which the ratio of the nickel content to the total content of all metal elements is 60 mol% or more in an air atmosphere; and a step for mixing the oxide with a Li-containing compound, and a step in which the obtained mixture is calcined in an air atmosphere and converted into a lithium composite oxide having a layered rock salt structure. In the oxide of the spinel structure main body, the peak integrated intensity ratio between the (003) plane and the (440) plane is 1.5 or less and the peak integrated intensity ratio between the (440) plane and the (311) plane is 4.5 or more as determined by X-ray powder diffraction measurement using a CuK [alpha] ray.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a positive electrode active material. Background Art

[0002] In recent years, lithium-ion secondary batteries have been used as portable power sources for personal computers, mobile terminals, etc., and as power sources for driving vehicles such as electric vehicles (BEV), hybrid electric vehicles (HEV), and plug-in hybrid electric vehicles (PHEV).

[0003] In the application of vehicle driving power source, lithium ion secondary batteries are required to have higher capacity from the viewpoint of extending the cruising range. A representative of the positive electrode active material of known lithium ion secondary batteries is a lithium composite oxide containing nickel. By using a lithium composite oxide with a high nickel content, the capacity of lithium ion secondary batteries can be increased (for example, refer to Patent Document 1).

[0004] When manufacturing a lithium composite oxide with a high nickel content, in order to suppress the mixing of divalent nickel cations, the precursor of the lithium composite oxide (particularly a composite hydroxide) and a lithium source are usually calcined in an oxygen atmosphere (i.e., an atmosphere with a higher oxygen concentration than the air). In Patent Document 1, from the viewpoint of reducing manufacturing costs, in order to reduce oxygen consumption, a nickel-cobalt-manganese composite hydroxide and a lithium source are pre-calcined once in an oxygen atmosphere, and then the pre-calcined product is mainly calcined in an air atmosphere.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Publication No. 2022-517078 Summary of the invention

[0008] However, in the method described in patent document 1, oxygen atmosphere is still needed in a pre-calcination. Thus, there is still room for reducing manufacturing costs, and preparing an oxygen atmosphere leads to a decrease in productivity. In addition, since excessive oxygen inhibits the crystal growth of lithium composite oxides, a higher calcination temperature is required, which also leads to a decrease in productivity in this regard. Therefore, it is desirable to develop a method for manufacturing a lithium composite oxide (i.e., positive electrode active material) with a high nickel content without using an oxygen atmosphere. In addition, it is particularly desirable that lithium ion secondary batteries have a high output in the application of power sources for vehicle driving.

[0009] Therefore, an object of the present invention is to provide a method for producing a positive electrode active material having a high nickel content and capable of providing a lithium ion secondary battery with high output without using an oxygen atmosphere.

[0010] The method for producing a positive electrode active material disclosed herein comprises the following steps: a step of heat-treating a hydroxide having a nickel content of 60 mol% or more to the total content of all metal elements in an atmospheric atmosphere to obtain an oxide having a spinel structure as a main component, a step of mixing the oxide with a Li-containing compound, and a step of calcining the obtained mixture in an atmospheric atmosphere to convert the oxide into a lithium composite oxide having a layered rock salt structure. In the oxide having a spinel structure as a main component, the peak integrated intensity ratio of the (003) plane to the (440) plane determined by X-ray powder diffraction using CuKα rays is 1.5 or less, and the peak integrated intensity ratio of the (440) plane to the (311) plane is 4.5 or more.

[0011] According to such a configuration, a positive electrode active material having a high nickel content and capable of providing a lithium ion secondary battery with high output can be produced without using an oxygen atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a flowchart showing each step of a method for producing a positive electrode active material according to one embodiment of the present invention.

[0013] Figure 2 It is a cross-sectional view schematically showing the structure of a lithium ion secondary battery constructed using a positive electrode active material obtained by the production method according to one embodiment of the present invention.

[0014] Figure 3 Yes means Figure 2 Schematic diagram of the exploded structure of the wound electrode body. DETAILED DESCRIPTION

[0015] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. It should be noted that matters not mentioned in this specification and required for the implementation of the present invention can be understood as design matters of a person skilled in the art based on the prior art in the art. The present invention can be implemented according to the contents disclosed in this specification and the technical common sense in the art. In addition, in the following drawings, components and parts having the same function are marked with the same symbols for explanation. In addition, the dimensional relationships (length, width, thickness, etc.) in each figure do not reflect the actual dimensional relationships. It should be noted that in this specification, the numerical range represented as "A to B" includes A and B.

[0016] It should be noted that in this specification, "secondary battery" refers to a storage device that can be repeatedly charged and discharged. In addition, in this specification, "lithium ion secondary battery" refers to a secondary battery that uses lithium ions as charge carriers and realizes charge and discharge through the transfer of charges accompanying lithium ions between positive and negative electrodes.

[0017] like Figure 1As shown, the method for producing the positive electrode active material according to the present embodiment includes the following steps: a step of heat-treating a hydroxide having a nickel content of 60 mol% or more to the total content of all metal elements in an atmospheric atmosphere to obtain an oxide having a spinel structure as the main body (hereinafter also referred to as a "heat treatment step") S101; a step of mixing the oxide with a Li-containing compound (hereinafter also referred to as a "mixing step") S102; and a step of calcining the obtained mixture in an atmospheric atmosphere to convert it into a lithium composite oxide having a layered rock salt structure (hereinafter also referred to as a "calcination step") S103. Among them, in the oxide having a spinel structure as the main body, the peak integrated intensity ratio of the (003) plane to the (440) plane determined by X-ray powder diffraction measurement is less than 1.5, and the peak integrated intensity ratio of the (440) plane to the (311) plane is greater than 4.5. The following describes in detail the various steps of the method for producing the positive electrode active material according to the present embodiment.

[0018] In the heat treatment step S101 , a hydroxide having a nickel content of 60 mol % or more relative to the total content of all metal elements is heat treated in an air atmosphere to obtain an oxide mainly having a spinel structure.

[0019] The hydroxide used as the raw material is a nickel-containing hydroxide, typically a hydroxide that has been used as a precursor when manufacturing lithium composite oxides (therefore, the hydroxide is also referred to as a "precursor hydroxide" below). The higher the nickel content, the higher the capacity of the lithium ion secondary battery can be, so in the hydroxide, the ratio of the nickel content to the total content of all metal elements is preferably 80 mol% or more.

[0020] The precursor hydroxide typically has Ni a Me b (OH)2 (wherein Me is a metal element or a semi-metal element other than Ni (for example, Co, Mn, Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, Sn, B, Si, etc.), a+b=1, a satisfies 0.60≤a≤1.00 (preferably 0.80≤a≤1.00), and b satisfies 0≤b≤0.40 (preferably 0≤b≤0.20)). The precursor hydroxide is, for example, a nickel-cobalt-manganese composite hydroxide, a nickel-cobalt-aluminum composite hydroxide, etc., preferably a nickel-cobalt-manganese composite hydroxide. In the present specification, the nickel-cobalt-manganese composite hydroxide may be doped with elements other than Ni, Co, Mn, O and H (especially metal elements and semi-metal elements), for example, having a composition represented by the following formula (I).

[0021] Ni x Co y Mn z M α(OH)2(I)

[0022] In formula (I), x, y, z and α each satisfy 0.60≤x<1.00, 0<y<0.40, 0<z<0.40, 0≤α≤0.10, and x+y+z=1. M is at least one element selected from Zr, Mo, W, Mg, Ca, Na, Fe, Cr, Zn, Sn, B and Al. x preferably satisfies 0.80≤x<1.00, and more preferably satisfies 0.80≤x≤0.90. y preferably satisfies 0.05≤y≤0.15. z preferably satisfies 0.05≤z≤0.15. α preferably satisfies 0≤α≤0.05.

[0023] The average particle size of the hydroxide is not particularly limited, and is, for example, 0.05 μm to 20 μm, preferably 2 μm to 10 μm. The average particle size of the hydroxide can be determined by taking a scanning electron microscope (SEM) photograph of hydroxide particles and calculating the average particle size of 100 particles selected at random.

[0024] The precursor hydroxide can be prepared by a known method (e.g., crystallization method). Specifically, for example, an aqueous solution of a nickel source compound (e.g., nickel sulfate) and other metal source compounds (e.g., sulfates of other metals) can be prepared, and a crystallization reaction is performed according to a known method using an aqueous solution containing an ammonium ion donor (e.g., ammonia water) and an alkaline aqueous solution (e.g., sodium hydroxide aqueous solution) to obtain a precursor hydroxide.

[0025] In the heat treatment step S101, the precursor hydroxide is heat treated in an air atmosphere to obtain an oxide of a spinel structure main body (hereinafter also referred to as a "precursor oxide"). Therefore, in the heat treatment step S101, the precursor hydroxide is converted into a precursor oxide by heat treatment in an air atmosphere.

[0026] Here, the crystal structure of the precursor oxide is mainly a spinel structure. When an X-ray powder diffraction (XRD) measurement using CuKα rays is performed, for the spinel structure, a peak of the (440) plane appears in the Miller index (hlk), and for the layered rock salt structure, peaks of the (003) plane and the (311) plane appear in the Miller index (hlk). Therefore, the crystal structure of the precursor oxide is mainly a spinel structure. In this embodiment, for the crystal structure of the precursor oxide, the peak integrated intensity ratio of the (003) plane to the (440) plane [(003) plane / (440) plane] obtained by using CuKα ray X-ray powder diffraction (XRD) measurement is less than 1.5, and the peak integrated intensity ratio of the (440) plane to the (311) plane [(440) plane / (311) plane] is greater than 4.5.

[0027] If the peak integrated intensity ratio [(003) plane / (440) plane] is greater than 1.5, sufficient output characteristics cannot be imparted to the lithium ion secondary battery. The peak integrated intensity ratio [(003) plane / (440) plane] is preferably 1.2 or less, and more preferably 1.0 or less.

[0028] If the peak integrated intensity ratio [(440) surface / (311) surface] is less than 4.5, sufficient output characteristics cannot be given to the lithium ion secondary battery. From the viewpoint of improving the effect of higher output, the peak integrated intensity ratio [(003) surface / (440) surface] is preferably 5.0 or more, more preferably 10 or more, further preferably 50 or more, particularly preferably 100 or more, and most preferably 200 or more.

[0029] In the precursor oxide, the crystallite diameter of the (440) plane determined by X-ray powder diffraction (XRD) measurement using CuKα rays is not particularly limited, but is preferably above.

[0030] It should be noted that X-ray powder diffraction (XRD) measurement can be performed according to a known method. Specifically, X-ray powder diffraction (XRD) measurement can be performed using CuKα rays using a known X-ray powder diffraction device. The calculation of the peak integrated intensity ratio can be performed according to a known method. Specifically, the calculation of the peak integrated intensity ratio can be performed using software attached to the device, etc.

[0031] The heat treatment conditions in the heat treatment step S101 are selected so that the precursor oxide satisfies the peak integrated intensity ratios obtained by powder XRD measurement.

[0032] As an indicator of the heat treatment conditions, there is a trend that the lower the heat treatment temperature, the greater the peak integrated intensity ratio [(003) plane / (440) plane], and there is a trend that the lower the heat treatment temperature, the greater the peak integrated intensity ratio [(440) plane / (311) plane]. There is a trend that the longer the heat treatment time, the greater the peak integrated intensity ratio [(440) plane / (311) plane]. The heat treatment temperature is preferably 400°C to 580°C, and more preferably 480°C to 550°C. The heat treatment time is preferably 0.1 hour to 120 hours, and more preferably 0.5 hour to 48 hours.

[0033] The heat treatment can be performed according to a known method. The heat treatment can be performed, for example, by using a continuous or batch electric furnace or the like. The precursor oxide of the spinel structure body can be obtained by heat treatment. In this embodiment, since the heat treatment step S101 is performed in an air atmosphere, there is no need to use an oxygen atmosphere.

[0034] It should be noted that the tap density of the precursor oxide of the spinel structure body obtained is higher than that of the precursor hydroxide. This is due to the influence of the separation of water from the precursor hydroxide. Therefore, more precursor oxides can be supplied in the calcining step S103, and from the perspective of high yield, the manufacturing method involved in this embodiment is advantageous.

[0035] Next, the mixing step S102 is described. In the mixing step S102, the obtained precursor oxide is mixed with the Li-containing compound. The mixing step S102 is the same as the conventional method and is usually performed under an air atmosphere. Therefore, an oxygen atmosphere may not be used. The mixing step S102 may be performed under a nitrogen atmosphere or an argon atmosphere.

[0036] The Li-containing compound can be a compound used as a known lithium source in the manufacture of the positive electrode active material, and specific examples thereof include lithium carbonate, lithium hydroxide, lithium nitrate, lithium acetate, lithium oxalate, lithium chloride, etc. These can be used alone or in combination of two or more. As the Li-containing compound, lithium hydroxide is preferred.

[0037] The mixing ratio of the precursor oxide and the Li-containing compound can be determined according to the composition required for the positive electrode active material. That is, the mixing ratio of the precursor oxide and the Li-containing compound is selected so that the molar ratio of the metal element contained in the precursor oxide to the Li element contained in the Li-containing compound is the same as the molar ratio of the metal element other than Li to the Li element in the composition required for the positive electrode active material.

[0038] The mixing can be performed by a known method. For example, the mixing can be performed using a known stirring device or mixing device such as a shaker mixer, a Loedige mixer, a Julia mixer, a V-type mixer, or a ball mill. The mixture can be prepared by the mixing.

[0039] Next, the calcination step S103 will be described. In the calcination step S103, the mixture is calcined in an air atmosphere to be converted into a lithium composite oxide having a layered rock salt structure.

[0040] Here, regarding the production of the positive electrode active material, when the precursor is a hydroxide having a layered rock salt structure and the lithium source is lithium hydroxide, the reaction formula in the calcination step is represented by the following formula (1) (It should be noted that in the following formula, M 1 is a metal element including Ni, etc.).

[0041] M 1 (OH)2+LiOH+1 / 4O2→LiM 1 O2+3 / 2H2O···(1)

[0042] On the other hand, when the precursor is an oxide having a layered rock salt structure, the reaction formula in the calcination step is represented by the following formula (2) (wherein, M 1 Same meaning as above).

[0043] M 1 O+LiOH+1 / 4O2→LiM 1 O2+1 / 2H2O···(2)

[0044] On the other hand, when the precursor is an oxide having a spinel crystal structure, the reaction formula in the calcination step is represented by the following formula (3) (wherein, M 1 Same meaning as above).

[0045] 1 / 3M 1 3O4+LiOH+1 / 12O2→LiM 1 O2+1 / 2H2O···(3)

[0046] It can be seen from the above formulas (1) to (3) that the precursor oxide having a spinel crystal structure has a high oxygen content, so the amount of oxygen required for the reaction is small (it should be noted that those skilled in the art can understand that the same applies even if the lithium source is other than lithium hydroxide). According to the comparison between formula (1) and formula (3), when using a precursor oxide having a spinel crystal structure, the amount of oxygen required is 1 / 3. Therefore, according to this embodiment, the synthesis reaction of the positive electrode active material can be carried out under the oxygen concentration contained in the atmospheric atmosphere. Therefore, in this embodiment, there is no need to use an oxygen atmosphere (i.e., an atmosphere with a higher oxygen concentration than the atmosphere). In addition, since a large amount of Ni exists in the precursor oxide in the form of trivalent, ion mixing can be suppressed, and thus, the obtained positive electrode active material can provide high output to the lithium ion secondary battery.

[0047] The calcination temperature and calcination time are not particularly limited as long as a lithium composite oxide with a layered rock salt structure is obtained. The calcination temperature is, for example, 700°C to 1000°C, preferably 750°C to 900°C, and more preferably 790°C to 900°C. The calcination time is, for example, 3 hours to 72 hours, preferably 4 hours to 24 hours, and more preferably 5 hours to 12 hours. In addition, the calcination is preferably carried out so that the crystallite diameter of the (003) plane determined by X-ray powder diffraction using CuKα rays in the obtained lithium composite oxide becomes It should be noted that if the calcination temperature is high, the crystallite diameter of the (003) plane tends to increase. In addition, if the calcination time is long, the crystallite diameter of the (003) plane tends to increase.

[0048] The mixture can be calcined by a known method. The calcination can be performed, for example, using a continuous or batch electric furnace. By calcining, a lithium composite oxide having a layered rock salt structure as a positive electrode active material can be obtained.

[0049] The obtained positive electrode active material (i.e., a lithium composite oxide with a layered rock salt structure) typically has Li 1+ c Ni a Me b O2 (wherein Me represents a metal element or semi-metal element other than Ni (for example, Co, Mn, Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, Sn, B, Si, etc.), a+b=1, c satisfies -0.05≤c≤0.30, a satisfies 0.60≤a≤1.00 (preferably 0.80≤a≤1.00), and b satisfies 0≤b≤0.40 (preferably 0≤b≤0.20)).

[0050] The positive electrode active material is, for example, a lithium nickel cobalt manganese composite oxide or a lithium nickel cobalt aluminum composite oxide, preferably a lithium nickel cobalt manganese composite oxide. In this specification, the lithium nickel cobalt manganese composite oxide may be doped with elements other than Li, Ni, Co, Mn and O (particularly metal elements or semi-metal elements), for example, having a composition represented by the following formula (II).

[0051] Li 1+t Ni x Co y Mn z M α O2(II)

[0052] In formula (II), t, x, y, z and α each satisfy -0.05≤t≤0.30, 0.60≤x<1.00, 0<y<0.40, 0<z<0.40, 0≤α≤0.10, and x+y+z=1. M is at least one element selected from Zr, Mo, W, Mg, Ca, Na, Fe, Cr, Zn, Sn, B and Al. t preferably satisfies 0≤t≤0.30. x preferably satisfies 0.80≤x<1.00, and more preferably satisfies 0.80≤x≤0.90. y preferably satisfies 0.05≤y≤0.15. z preferably satisfies 0.05≤z≤0.15. α preferably satisfies 0≤α≤0.05.

[0053] From the viewpoint of a higher output improvement effect, in the positive electrode active material, the crystallite diameter of the (003) plane determined by X-ray powder diffraction measurement using CuKα rays is preferably More preferably It should be noted that the crystallite diameter of the (003) plane can be measured by a known method. Specifically, for example, the crystallite diameter can be obtained by performing X-ray powder diffraction measurement by the above method and using the half width (half peak width) of the (003) plane, 2θ value and Scherrer formula.

[0054] The average particle size of the positive electrode active material is not particularly limited, and is, for example, 0.05 μm to 20 μm, preferably 2 μm to 10 μm. It should be noted that the average particle size of the positive electrode active material can be obtained by taking a scanning electron microscope (SEM) photograph of the particles of the positive electrode active material and finding the average particle size of 100 particles selected at random.

[0055] The positive electrode active material obtained by the manufacturing method involved in this embodiment has a high nickel content. Therefore, when a lithium ion secondary battery is constructed using the positive electrode active material, the capacity of the lithium ion secondary battery is high. In addition, the output characteristics of the lithium ion secondary battery using the positive electrode active material are also excellent. Therefore, the positive electrode active material involved in this embodiment is suitable as a positive electrode active material for a lithium ion secondary battery.

[0056] Then, a specific configuration example of a lithium ion secondary battery using the positive electrode active material obtained by the production method according to the present embodiment described above will be described with reference to the drawings.

[0057] Figure 2 The lithium-ion secondary battery 100 shown is a sealed battery constructed by accommodating a flat-shaped wound electrode body 20 and a non-aqueous electrolyte (not shown) in a flat square battery case (i.e., an outer container) 30. A positive terminal 42 and a negative terminal 44 for external connection and a thin-walled safety valve 36 are provided in the battery case 30, and the safety valve 36 is set to release the internal pressure when the internal pressure of the battery case 30 rises to a specified level or above. In addition, an injection port (not shown) for injecting a non-aqueous electrolyte is provided in the battery case 30. The positive terminal 42 is electrically connected to the positive electrode collector plate 42a. The negative terminal 44 is electrically connected to the negative electrode collector plate 44a. As the material of the battery case 30, for example, a light and thermally conductive metal material such as aluminum can be used.

[0058] like Figure 2 and Figure 3As shown, the wound electrode body 20 has a form in which a positive electrode sheet 50 and a negative electrode sheet 60 are stacked and wound in the long-side direction with two long-strip separator sheets 70 interposed therebetween. The positive electrode sheet 50 has a structure in which a positive electrode active material layer 54 is formed on one side or both sides (here both sides) of a long-strip positive electrode collector 52 along the long-side direction. The negative electrode sheet 60 has a structure in which a negative electrode active material layer 64 is formed on one side or both sides (here both sides) of a long-strip negative electrode collector 62 along the long-side direction. The positive electrode active material layer non-formed portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode collector 52 is exposed) and the negative electrode active material layer non-formed portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode collector 62 is exposed) are formed to protrude outward from both ends of the winding axis direction (i.e., the sheet width direction orthogonal to the above-mentioned long-side direction) of the wound electrode body 20. The positive electrode current collector plate 42a and the negative electrode current collector plate 44a are joined to the positive electrode active material layer non-formed portion 52a and the negative electrode active material layer non-formed portion 62a, respectively.

[0059] As the positive electrode collector 52 constituting the positive electrode sheet 50, a known positive electrode collector used in a lithium ion secondary battery can be used, and examples thereof include sheets or foils made of a metal having good conductivity (for example, aluminum, nickel, titanium, stainless steel, etc.). As the positive electrode collector 52, aluminum foil is preferred.

[0060] The size of the positive electrode current collector 52 is not particularly limited and can be appropriately determined according to the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness thereof is not particularly limited, and is, for example, 5 μm to 35 μm, and preferably 7 μm to 20 μm.

[0061] The positive electrode active material layer 54 contains a positive electrode active material. The positive electrode active material uses at least the positive electrode active material obtained by the manufacturing method involved in the present embodiment described above. The content of the positive electrode active material is not particularly limited, and is preferably 70% by mass or more in the positive electrode active material layer 54 (that is, relative to the total mass of the positive electrode active material), more preferably 80% by mass or more, and further preferably 85% by mass or more.

[0062] The positive electrode active material layer 54 may contain components other than the positive electrode active material, and examples thereof include lithium phosphate (Li 3 PO 4 ), a conductive material, and a binder.

[0063] The content of lithium phosphate in the positive electrode active material layer 54 is not particularly limited, but is preferably 1% by mass to 15% by mass, and more preferably 2% by mass to 12% by mass.

[0064] As the conductive material, for example, carbon black such as acetylene black (AB) or other carbon materials (for example, graphite, etc.) can be preferably used. The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, and is, for example, 0.1 mass % to 20 mass %, preferably 1 mass % to 15 mass %, and more preferably 2 mass % to 10 mass %.

[0065] As the binder, for example, polyvinylidene fluoride (PVdF) can be used. The content of the binder in the positive electrode active material layer 54 is not particularly limited, and is, for example, 0.5 to 15 mass %, preferably 1 to 10 mass %, and more preferably 1.5 to 8 mass %.

[0066] The thickness of the positive electrode active material layer 54 is not particularly limited, and is, for example, 10 μm to 300 μm, and preferably 20 μm to 200 μm.

[0067] As the negative electrode collector 62 constituting the negative electrode sheet 60, a known negative electrode collector used in a lithium ion secondary battery can be used, and examples thereof include sheets or foils made of a metal having good conductivity (for example, copper, nickel, titanium, stainless steel, etc.). As the negative electrode collector 62, copper foil is preferred.

[0068] The size of the negative electrode current collector 62 is not particularly limited and can be appropriately determined according to the battery design. When copper foil is used as the negative electrode current collector 62, the thickness thereof is not particularly limited, and is, for example, 5 μm to 35 μm, and preferably 7 μm to 20 μm.

[0069] The negative electrode active material layer 64 contains a negative electrode active material. As the negative electrode active material, for example, carbon materials such as graphite, hard carbon, and soft carbon can be used. The graphite can be natural graphite or artificial graphite, and the graphite can be amorphous carbon-coated graphite in a form coated with an amorphous carbon material.

[0070] The average particle size (median particle size D50) of the negative electrode active material is not particularly limited, and is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm.

[0071] The content of the negative electrode active material in the negative electrode active material layer 64 is not particularly limited, but is preferably 90% by mass or more, and more preferably 95% by mass or more.

[0072] The negative electrode active material layer 64 may contain components other than the negative electrode active material, such as a binder, a thickener, and the like.

[0073] As the binder, for example, styrene-butadiene rubber (SBR) and its modified bodies, nitrile rubber and its modified bodies, acrylic rubber and its modified bodies, fluororubber, etc. can be used. Among them, SBR is preferred. The content of the binder in the negative electrode active material layer 64 is not particularly limited, preferably 0.1 mass % to 8 mass %, more preferably 0.2 mass % to 3 mass %.

[0074] As the thickener, for example, cellulose polymers such as carboxymethyl cellulose (CMC), methyl cellulose (MC), cellulose acetate phthalate (CAP), and hydroxypropyl methyl cellulose (HPMC); polyvinyl alcohol (PVA) and the like can be used. Among them, CMC is preferred. The content of the thickener in the negative electrode active material layer 64 is not particularly limited, but is preferably 0.3% to 3% by mass, and more preferably 0.4% to 2% by mass.

[0075] The thickness of the negative electrode active material layer 64 is not particularly limited, and is, for example, 10 μm to 300 μm, and preferably 20 μm to 200 μm.

[0076] As the separator 70, for example, a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, polyamide, etc. can be cited. The porous sheet can be a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which PP layers are laminated on both sides of a PE layer). A heat-resistant layer (HRL) can be provided on the surface of the separator 70.

[0077] The thickness of the spacer 70 is not particularly limited, and is, for example, 5 μm to 50 μm, and preferably 10 μm to 30 μm.

[0078] The non-aqueous electrolyte typically contains a non-aqueous solvent and an electrolyte salt (in other words, a supporting salt). As the non-aqueous solvent, various organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones used in the electrolyte of a general lithium-ion secondary battery can be used without particular limitation. Among them, carbonates are preferred, and as specific examples, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), dimethyl trifluorocarbonate (TFDMC), etc. can be illustrated. Such a non-aqueous solvent can be used alone or in combination of two or more.

[0079] As the electrolyte salt, for example, lithium salts such as LiPF6, LiBF4, and lithium bis(fluorosulfonyl)imide (LiFSI) can be used, among which LiPF6 is preferred. The concentration of the electrolyte salt is not particularly limited, but is preferably 0.7 mol / L to 1.3 mol / L.

[0080] It should be noted that the non-aqueous electrolyte may contain components other than the above-mentioned components, for example, film formers such as oxalate complexes, gas generators such as biphenyl (BP) and cyclohexylbenzene (CHB), and various additives such as thickeners, as long as the effects of the present invention are not significantly impaired.

[0081] The capacity of the lithium ion secondary battery 100 is high and the output characteristics are excellent. The lithium ion secondary battery 100 can be used for various purposes. As suitable uses, a driving power supply carried in vehicles such as electric vehicles (BEV), hybrid electric vehicles (HEV), and plug-in hybrid electric vehicles (PHEV) can be cited. In addition, the lithium ion secondary battery 100 can be used as a storage battery for a small power storage device, etc. The lithium ion secondary battery 100 can typically be used in the form of a battery pack formed by connecting a plurality of batteries in series and / or in parallel.

[0082] In the above, a square lithium-ion secondary battery having a flat wound electrode body is used as an example for explanation. However, the positive electrode active material obtained by the manufacturing method involved in the present embodiment can also be used for other types of lithium-ion secondary batteries according to a known method. For example, the positive electrode active material obtained by the manufacturing method involved in the present embodiment can also be used to construct a lithium-ion secondary battery having a stacked electrode body (that is, an electrode body formed by alternating stacking of multiple positive electrodes and multiple negative electrodes). In addition, the positive electrode active material obtained by the manufacturing method involved in the present embodiment can also be used to construct a cylindrical lithium-ion secondary battery, a coin-type lithium-ion secondary battery, a laminated lithium-ion secondary battery, etc. In addition, the positive electrode active material obtained by the manufacturing method involved in the present embodiment can also be used to construct an all-solid secondary battery in which the electrolyte is a solid electrolyte.

[0083] Hereinafter, examples according to the present invention will be described, but the present invention is not limited to the contents shown in these examples.

[0084] [Example 1]

[0085] A composite hydroxide containing nickel, cobalt and manganese in a molar ratio of 8:1:1 (i.e., Ni 0.8 Co 0.1 Mn 0.1 (OH)2) as a raw material precursor hydroxide. The precursor hydroxide was heat treated at 550°C in an air atmosphere for 0.5 hours. Thus, a precursor oxide was obtained. The crystal structure of the precursor oxide was analyzed by the method described below.

[0086] The obtained precursor oxide is mixed with lithium hydroxide. The metal element in the precursor oxide and the lithium element in the lithium hydroxide are mixed in a molar ratio of 1:1. The obtained mixture is calcined in an electric furnace at 850° C. for 10 hours under an air atmosphere to obtain a lithium composite oxide as a positive electrode active material.

[0087] [Examples 2 to 18]

[0088] Using the composite hydroxide of the composition shown in Table 1, heat treatment is performed in an air atmosphere at the heat treatment temperature and heat treatment time shown in Table 1 to obtain a precursor oxide. The crystal structure of the precursor oxide is analyzed by the method described later. The precursor oxide is mixed with lithium hydroxide. The mixture is mixed in a manner such that the metal element in the precursor oxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined in an electric furnace at the calcination temperature and calcination time shown in Table 2 in an air atmosphere to obtain a lithium composite oxide as a positive electrode active material.

[0089] [Comparative Example 1]

[0090] As a raw material, Ni 0.8 Co 0.1 Mn 0.1 A precursor hydroxide of a composition represented by (OH)2 is prepared. The precursor hydroxide is mixed with lithium hydroxide. The mixture is mixed in such a way that the metal element in the precursor hydroxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined in an electric furnace at 850°C for 10 hours under an atmospheric atmosphere to obtain a lithium composite oxide.

[0091] [Comparative Example 2]

[0092] As a raw material, Ni 0.8 Co 0.1 Mn 0.1 A precursor hydroxide of a composition represented by (OH)2 is prepared. The precursor hydroxide is mixed with lithium hydroxide. The mixture is mixed in such a way that the metal element in the precursor hydroxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined at 860°C for 10 hours in an oxygen atmosphere in an electric furnace to obtain a lithium composite oxide.

[0093] [Comparative Examples 3 to 5]

[0094] Use Ni 0.8 Co 0.1 Mn 0.1(OH)2, heat-treated in an atmospheric atmosphere at a heat treatment temperature and heat treatment time shown in Table 1 to obtain a precursor oxide. The crystal structure of the precursor oxide is analyzed by the method described later. The precursor oxide is mixed with lithium hydroxide. The mixture is mixed in a manner such that the metal element in the precursor oxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined in an electric furnace at a calcination temperature and calcination time shown in Table 2 in the atmosphere shown in Table 2 to obtain a lithium composite oxide as a positive electrode active material.

[0095] [Comparative Example 6]

[0096] As a raw material, Ni 0.6 Co 0.2 Mn 0.2 A precursor hydroxide of a composition represented by (OH)2 is prepared. The precursor hydroxide is mixed with lithium hydroxide. The mixture is mixed in such a way that the metal element in the precursor hydroxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined in an electric furnace at 890° C. for 10 hours under an atmospheric atmosphere to obtain a lithium composite oxide.

[0097] [Comparative Example 7]

[0098] As a raw material, Ni 0.6 Co 0.2 Mn 0.2 A precursor hydroxide of a composition represented by (OH)2 is prepared. The precursor hydroxide is mixed with lithium hydroxide. The mixture is mixed in such a way that the metal element in the precursor hydroxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined at 900°C for 10 hours in an electric furnace under an oxygen atmosphere to obtain a lithium composite oxide.

[0099] [Comparative Example 8]

[0100] As a raw material, Ni 0.8 Co 0.1 Mn 0.1 A precursor hydroxide of a composition represented by (OH)2 is prepared. The precursor hydroxide is mixed with lithium hydroxide. The metal element in the precursor hydroxide and the lithium element in the lithium hydroxide are mixed in a molar ratio of 1:1. The obtained mixture is pre-calcined at 500°C for 5 hours in an oxygen atmosphere in an electric furnace, and then calcined at 850°C for 10 hours in an air atmosphere to obtain a lithium composite oxide.

[0101] [Comparative Example 9]

[0102] When nickel sulfate, cobalt sulfate and manganese sulfate are used to prepare the precursor by crystallization, sodium persulfate and sodium peroxide are added to obtain Ni 0.6 Co 0.2 Mn0.2 O(OH) is used as a raw material precursor oxyhydroxide. The precursor oxyhydroxide is mixed with lithium hydroxide. The mixture is mixed in such a way that the metal element in the precursor oxyhydroxide and the lithium element in the lithium hydroxide have a molar ratio of 1:1. The obtained mixture is calcined at 890° C. for 10 hours in an electric furnace under an atmospheric atmosphere to obtain a lithium composite oxide.

[0103] [X-ray powder diffraction measurement of precursor oxide]

[0104] The precursor oxide obtained by the heat treatment was subjected to XRD powder measurement using an XRD device "smart Lab" (manufactured by Rigaku Corporation). The peak integrated intensity ratio of the (003) plane to the (440) plane [(003) plane / (440) plane] and the peak integrated intensity ratio of the (440) plane to the (311) plane [(440) plane / (311) plane] of the Miller index hlk were calculated using the analysis software "PDXL2" (manufactured by Rigaku Corporation). The results are shown in Table 1.

[0105] [X-ray powder diffraction measurement of positive electrode active material]

[0106] The positive electrode active material obtained above was subjected to XRD powder measurement using an XRD device "smart Lab" (manufactured by Rigaku Corporation). The crystallite diameter of the (003) plane was calculated using the half width, 2θ value and Scherrer formula of the (003) plane using the analysis software "PDXL2" (manufactured by Rigaku Corporation). The results are shown in Table 2.

[0107] [Determination of tap density of precursor oxides and precursor hydroxides]

[0108] The precursor hydroxide (Ni) used in Examples 1 to 6, 9 to 18 and Comparative Examples 1 to 5 and 8 was measured using a commercially available Tapping Machine "KRS-409" (manufactured by Kuramochi Scientific Instruments Co., Ltd.) according to the method specified in JIS K1469: 2003. 0.8 Co 0.1 Mn 0.1 (OH)2), and the tap density of the precursor oxides prepared in Examples 1 to 6 and 9 to 18. As a result, the tap density of the precursor oxides was greater than that of the precursor hydroxides. The tap density of the precursor hydroxides (Ni 0.6 Co 0.2 Mn 0.2 (OH)2), and the tap density of the precursor oxide prepared in Example 7, the tap density of the precursor oxide is greater than that of the precursor hydroxide.

[0109] <Production of lithium-ion secondary battery for evaluation>

[0110] The positive electrode active material of each embodiment and each comparative example prepared above, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in N-methylpyrrolidone (NMP) at a mass ratio of positive electrode active material: AB: PVDF = 85: 10: 5 to prepare a paste for forming a positive electrode active material layer. The paste was applied on an aluminum foil with a thickness of 15 μm and dried to prepare a positive electrode sheet.

[0111] Natural graphite (C) as a negative electrode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in ion exchange water at a mass ratio of C:SBR:CMC=98:1:1 to prepare a paste for forming a negative electrode active material layer. The paste was applied on a copper foil with a thickness of 10 μm and dried to prepare a negative electrode sheet.

[0112] In addition, as a separator sheet, a porous polyolefin sheet having a three-layer structure of PP / PE / PP and a thickness of 20 μm was prepared.

[0113] The positive electrode sheet, negative electrode sheet and separator sheet are overlapped, and the electrode terminals are installed and housed in a laminated shell. Next, a non-aqueous electrolyte is injected into the laminated shell to seal the laminated shell airtightly. It should be noted that the non-aqueous electrolyte is a solution made by dissolving LiPF6 as a supporting salt at a concentration of 1.0 mol / L in a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:4:3. The lithium-ion secondary battery for evaluation is obtained in the above manner.

[0114] <Output Characteristics Evaluation>

[0115] After activation treatment, each evaluation lithium ion secondary battery was adjusted to SOC 60% and placed in an environment of -10°C. Each evaluation lithium ion secondary battery was discharged at a current value of 15C for 2 seconds. The output power (W) was calculated based on the voltage and current value at this time. When the output power of the evaluation lithium ion secondary battery using the positive electrode active material obtained in Comparative Example 1 is set to 100, the ratio of the output power of the evaluation lithium ion secondary battery using the positive electrode active material obtained in other comparative examples and embodiments is calculated. The results are shown in Table 2.

[0116] [Table 1]

[0117]

[0118] [Table 2:

[0119]

[0120] According to the results of Tables 1 and 2, it is known that by heat treating a hydroxide having a nickel content of 60 mol % or more under an atmospheric atmosphere and converting it into an oxide having a spinel structure main body with a peak integrated intensity ratio [(003) face / (440) face] of less than 1.5 and a peak integrated intensity ratio [(440) face / (311) face] of more than 4.5, it is possible to manufacture a positive electrode active material that can give a high output to a lithium ion secondary battery without using an oxygen atmosphere. Therefore, it is known that according to the manufacturing method of the positive electrode active material disclosed herein, a positive electrode active material that can give a high output to a lithium ion secondary battery and has a high nickel content can be manufactured without using an oxygen atmosphere.

[0121] The specific examples of the present invention have been described in detail above, but these are merely examples and do not limit the scope of the claims. The technology described in the scope of the claims includes various modifications and changes of the specific examples described above.

[0122] That is, the method for producing a positive electrode active material disclosed herein is the following items [1] to [5].

[0123] [1] A method for producing a positive electrode active material, comprising the following steps:

[0124] A step of heat-treating a hydroxide having a nickel content of 60 mol % or more to the total content of all metal elements in an air atmosphere to obtain an oxide having a spinel structure as a main component,

[0125] a step of mixing the oxide with a Li-containing compound, and

[0126] The obtained mixture is calcined in an air atmosphere to convert it into a lithium composite oxide having a layered rock salt structure.

[0127] In the oxide of the spinel structure main body, the peak integrated intensity ratio between the (003) plane and the (440) plane determined by X-ray powder diffraction measurement using CuKα rays is less than 1.5, and the peak integrated intensity ratio between the (440) plane and the (311) plane is greater than 4.5.

[0128] [2] The production method according to item [1], wherein the ratio of the content of nickel to the total content of all metal elements in the hydroxide is 80 mol% or more.

[0129] [3] The production method according to item [1] or [2], wherein the hydroxide is a nickel-cobalt-manganese composite hydroxide, and the layered rock salt structured lithium composite oxide is a lithium-nickel-cobalt-manganese composite oxide.

[0130] [4] The production method according to any one of items [1] to [3], wherein the peak integrated intensity ratio of the above-mentioned (440) plane and (311) plane is greater than 10.

[0131] [5] The production method according to any one of items [1] to [4], wherein the crystallite diameter of the (003) plane of the layered rock salt structure lithium composite oxide determined by X-ray powder diffraction using CuKα rays is

Claims

1. A method for producing a positive electrode active material, comprising the following steps: A step of heat-treating a hydroxide having a nickel content of 60 mol % or more to the total content of all metal elements in an air atmosphere to obtain an oxide having a spinel structure as a main component, a step of mixing the oxide with a Li-containing compound, and The obtained mixture is calcined in an air atmosphere to convert it into a lithium composite oxide having a layered rock salt structure. In the oxide of the spinel structure main body, the peak integrated intensity ratio of the (003) plane to the (440) plane determined by X-ray powder diffraction measurement using CuKα rays is less than 1.5, and the peak integrated intensity ratio of the (440) plane to the (311) plane is greater than 4.

5.

2. The manufacturing method according to claim 1, wherein: In the hydroxide, the ratio of the content of nickel to the total content of all metal elements is 80 mol % or more.

3. The manufacturing method according to claim 1, wherein: The hydroxide is a nickel-cobalt-manganese composite hydroxide, and the lithium composite oxide with a layered rock salt structure is a lithium-nickel-cobalt-manganese composite oxide.

4. The manufacturing method according to claim 1, wherein: The peak integrated intensity ratio of the (440) plane to the (311) plane is greater than 10.

5. The manufacturing method according to claim 1, wherein: In the layered rock salt structured lithium composite oxide, the crystallite diameter of the (003) plane determined by X-ray powder diffraction measurement using CuKα rays is