Microwave dielectric ceramic material with adjustable dielectric constant and preparation method thereof
By designing xMg2SiO4-(1-x)Mg2TiO4-0.09CaTiO3-0.005MO microwave dielectric ceramic material, the problem of uncontrollable frequency temperature coefficient is solved, and the flexible adjustment of dielectric constant and the stability of frequency temperature coefficient are achieved, which is suitable for Various antenna and filter applications.
Patent Information
- Application Number
- CN202410711492.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-04
AI Technical Summary
The frequency temperature coefficient of existing microwave dielectric materials with adjustable dielectric constant is uncontrollable, which limits its application scenarios. In particular, it is difficult to maintain the frequency temperature coefficient near zero when the dielectric constant changes, and cannot meet the market's requirements for different dielectric constants and temperatures. Coefficient change requirements.
Use microwave dielectric ceramic materials with a composition expression of xMg2SiO4-(1-x)Mg2TiO4-0.09CaTiO3-0.005MO, through pre-synthesized powder and secondary batching, ball milling and sintering Preparation, the dielectric constant is adjustable in the range of 10.0~19.9, the Q×f value is 47704~68149GHz, and the frequency temperature coefficient τf≤±10ppm/℃ ensures that the frequency temperature coefficient is close to zero at all stages.
It achieves flexible adjustment of the dielectric constant in the range of 10.0 to 19.9, while maintaining the stability of high quality factor and frequency temperature coefficient. It is suitable for laminated patch antennas, baseband antennas, navigation antennas and other fields.
Smart Images

Figure CN118724562A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microwave dielectric materials, and in particular to a microwave dielectric ceramic material with adjustable dielectric constant and a preparation method thereof. Background Art
[0002] The size of the dielectric constant affects the speed of signal transmission. A low dielectric constant can reduce the mutual coupling of electromagnetic signals and improve signal transmission and response speed. The lower the dielectric constant, the smaller the signal transmission delay. The high quality factor (Q value) can reduce the energy consumption during signal transmission and increase the frequency selectivity of the device. Therefore, in high-frequency signal systems, ceramic materials with low dielectric constants are of great significance in reducing signal delays.
[0003] When establishing a reliable data connection, antenna technology affects the performance of the transmission channel, the characteristics of the transceiver, and the selection of digital signal processing models. A printed antenna is an antenna in which both the radiator and the feed part are arranged on a dielectric substrate. Microstrip patch antenna is a common printed antenna. It has the advantages of light weight, convenient processing and flexible design, but the biggest disadvantage of patch antenna is its narrow bandwidth. As an improved structure of patch antenna, laminated patch antenna inherits the advantages of patch antenna and extends the antenna bandwidth. With the development and popularization of laminated patch antenna, there is an increasing demand for microwave dielectric materials with lower dielectric constants to adjust the dielectric constant at any time. It is very necessary and of great commercial value to develop microwave dielectric materials with low dielectric constants with adjustable dielectric constants, coordinate the frequency temperature coefficient and maintain a high Q value, so as to meet the market and RF designers' demand for changing dielectric constants at any time.
[0004] Yin Wang et al. disclosed a two-phase Mg with adjustable dielectric constant x Zn y Al2O 4-z The Sr2TiO4 microwave dielectric material has an adjustable dielectric constant between 8.5 and 18.63. However, since the designed material is just a two-phase composite with one positive and one negative frequency temperature coefficient, its frequency temperature coefficient varies within the range of -77 to +39ppm / ℃ as the dielectric constant changes, and can only be close to zero in a small range in the middle, which limits its application scenarios to a certain extent. Summary of the invention
[0005] The existing design of adjustable dielectric constant systems usually has the disadvantage of uncontrollable frequency temperature coefficient. Although the dielectric constant is adjustable, the frequency temperature coefficient can only be close to zero near a certain dielectric constant. If the frequency temperature coefficient needs to be close to zero near other adjustable dielectric constants, the formulation system needs to be redesigned. In order to cope with the rapid changes in market demand and to provide microwave dielectric ceramic material formulations with different dielectric constants and near-zero frequency temperature coefficients in a timely manner, the purpose of the present invention is to provide a microwave dielectric ceramic material with adjustable dielectric constant and a preparation method thereof. The dielectric constant of the prepared microwave dielectric material is adjustable in the range of 10 to 20, and its Q×f value (Q is the quality factor of the material, f is the resonant frequency) is 47704 to 68149 GHz, and the frequency temperature coefficient τ f ≤±10ppm / ℃.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A microwave dielectric ceramic material with adjustable dielectric constant has a composition expression of: xMg2SiO4-(1-x)Mg2TiO4-0.09CaTiO3-0.005MO, wherein: 0.15≤x≤0.7, and MO is an auxiliary agent.
[0008] The additive MO is an oxide or a mixture of oxides, wherein M is one or more of Fe, Zn, Nb, Si and Mg.
[0009] The dielectric constant of the microwave dielectric ceramic material is adjustable within the range of 10.0 to 19.9, and the Q×f value is 47704 to 68149 GHz; the frequency temperature coefficient τ f ≤±10ppm / ℃.
[0010] The two materials Mg2SiO4 and Mg2TiO4 in the microwave dielectric ceramic material have different dielectric constants, but similar frequency temperature coefficients, and both can coexist independently with CaTiO3 optimized by MO. This characteristic of the two materials Mg2SiO4 and Mg2TiO4 enables the prepared microwave dielectric ceramic material to achieve different dielectric constant changes and keep the frequency temperature coefficient close to zero in all stages.
[0011] The dielectric constant of the microwave dielectric ceramic material gradually increases as the value of x in its composition expression decreases.
[0012] The preparation method of the microwave dielectric ceramic material with adjustable dielectric constant is as follows: first, pre-synthesized powder I (Mg2SiO4-Mg2TiO4 phase) and pre-synthesized powder II (0.09CaTiO3-0.005MO) are prepared respectively; then, the pre-synthesized powder I and the pre-synthesized powder II are subjected to secondary batching to complete three-phase composite; finally, the microwave dielectric ceramic material with adjustable dielectric constant is obtained by ball milling and sintering.
[0013] The method specifically comprises the following steps:
[0014] (1) Ingredients: magnesium oxide, silicon dioxide, titanium dioxide, calcium carbonate and MO additive are used as raw materials. First, magnesium oxide, silicon dioxide and titanium dioxide are weighed according to the molar ratio of Mg, Si and Ti in Mg2SiO4 and Mg2TiO4 in the microwave dielectric ceramic material composition expression, and mixed evenly to obtain a mixture I. Then, titanium dioxide, calcium carbonate and MO additive are weighed according to the molar ratio of Ca, Ti and MO in CaTiO3 and MO in the microwave dielectric ceramic material composition expression, and mixed evenly to obtain a mixture II.
[0015] (2) Mixing: ball-milling and drying the mixed material I and the mixed material II obtained in step (1) to obtain dry powder material I and dry powder material II;
[0016] (3) Pre-sintering: placing the dry powder I and the dry powder II obtained in step (2) in different alumina crucibles, respectively, and pre-sintering them in a carbon rod furnace to obtain pre-synthesized powder I and pre-synthesized powder II;
[0017] (4) Secondary batching: weigh and mix the pre-synthesized powder I (x Mg2SiO4-(1-x)Mg2TiO4) and pre-synthesized powder II (0.09CaTiO3-0.005MO) obtained in step (3) according to the composition of the microwave dielectric ceramic material to obtain secondary raw material powder;
[0018] (5) slurry preparation: the secondary raw material powder obtained in step (4) is ball-milled for 20 to 26 hours, with the ball-milling medium being zirconium balls and deionized water, to obtain a viscous slurry;
[0019] (6) Molding: Add a binder (polyvinyl alcohol solution) accounting for 5 to 20 wt% of the slurry obtained in step (5), then perform spray granulation and compression molding in sequence, and finally sinter in a carbon rod furnace to obtain the microwave dielectric ceramic material with adjustable dielectric constant.
[0020] Furthermore, in step (2), during the ball milling process, the ball milling medium is zirconium balls and deionized water; after ball milling, the product is placed in an oven at 150° C. and dried for 12 hours.
[0021] Furthermore, in step (3), the pre-firing temperature in the carbon rod furnace is 1000° C. to 1200° C., and the pre-firing time is 2 to 4 hours.
[0022] Furthermore, in step (6), the sintering temperature in the carbon rod furnace is 1250° C. to 1300° C., and the sintering time is 3 hours.
[0023] The advantages and beneficial effects of the present invention are as follows:
[0024] 1. In the formula design of the microwave dielectric ceramic material of the present invention, the CaTiO3-yMO part in the composition expression is first pre-synthesized separately, so that the single-phase CaTiO3 can reduce the pre-synthesis temperature and control the titanium reduction phenomenon with the help of the MO additive, and then it is three-phase composited with the other part x Mg2SiO4-(1-x)Mg2TiO4 in the pre-synthesized expression, so that the three phases after the composite exist independently and exert their own performance.
[0025] 2. The Mg2SiO4 phase and Mg2TiO4 phase in the material formula of the present invention are the preferred phase system, which has the characteristics of different dielectric constants, similar frequency temperature coefficients and non-reaction with each other, so that the dielectric constant can be linearly adjusted by only changing the ratio of the two phases, while ensuring that the frequency temperature coefficient is close to zero throughout the process.
[0026] 3. A specific amount of CaTiO3 (the amount introduced accounts for 9% of the total molar amount of Mg2SiO4 and Mg2TiO4) is introduced into the formula of the present invention. The introduction ratio is uniquely designed and repeatedly verified, and can meet the near-zero control of the frequency temperature coefficient in the overall material system when the x value changes from 0.15 to 0.7.
[0027] 4. The microwave dielectric material with adjustable dielectric constant of the present invention has a dielectric constant adjustable in the range of 10.0 to 19.9, a Q×f value of 47704 to 68149 GHz, and a frequency temperature coefficient τ f ≤±10ppm / ℃, can be widely used in laminated patch antennas, baseband antennas, navigation antennas, dielectric waveguide filters and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the X-ray diffraction pattern of the microwave dielectric ceramic material prepared in Example 1-6. DETAILED DESCRIPTION
[0029] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously in conjunction with the embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0030] Embodiment 1-6:
[0031] The composition expression of the microwave dielectric ceramic material in the present invention is: xMg2SiO4-(1-x)Mg2TiO4-0.09CaTiO3-0.005MO, wherein: 0.15≤x≤0.7, MO is an additive. The additive MO is an oxide mixture composed of Fe, Zn, Nb, Si, and Mg (M is one or more of Fe, Zn, Nb, Si, and Mg).
[0032] The values of x in the composition expressions of the microwave dielectric ceramic materials of Examples 1-6 are shown in Table 1.
[0033] The preparation method of the microwave dielectric ceramic material of Example 1-6 is as follows:
[0034] (1) Ingredients: Using magnesium oxide, silicon dioxide, titanium dioxide, calcium carbonate and MO additive as raw materials, firstly weigh magnesium oxide, silicon dioxide and titanium dioxide according to the molar ratio of Mg, Si and Ti in Mg2SiO4 and Mg2TiO4 in the microwave dielectric ceramic material expression (i.e., the molar ratio of Mg, Si and Ti is 2:x:(1-x)) and mix them evenly to obtain a mixture I, then weigh titanium dioxide, calcium carbonate and MO additive according to the molar ratio of Ca, Ti and MO in CaTiO3 and MO in the microwave dielectric ceramic material expression (i.e., the molar ratio of Ca, Ti and MO is 0.09:0.09:0.005) and mix them evenly to obtain a mixture II;
[0035] (2) Mixing: The mixed materials I and II are respectively subjected to ball milling treatment and dried to obtain dry powder I (xMg2SiO4-(1-x)Mg2TiO4) and dry powder II (0.09CaTiO3-0.005MO);
[0036] (3) Pre-sintering: The obtained dry powder I and dry powder II are placed in different alumina crucibles, and pre-sintered at 1100° C. in a carbon rod furnace to obtain pre-synthesized powder I (xMg2SiO4-(1-x)Mg2TiO4) and pre-synthesized powder II (0.09CaTiO3-0.005MO);
[0037] (4) secondary batching: weighing and mixing the pre-synthesized powder I and the pre-synthesized powder II according to the molar ratio in the composition expression of the microwave dielectric ceramic material to obtain a secondary raw material powder;
[0038] (5) Slurry preparation: The secondary raw material powder is ball-milled for 24 hours using zirconium balls and deionized water as the ball-milling media to obtain a viscous slurry;
[0039] (6) Molding: Add a binder accounting for 12 wt% of the slurry (polyvinyl alcohol solution with a concentration of 10 wt.%) to the slurry obtained in step (5), then perform spray granulation and press molding in sequence, and finally sinter at 1280°C in a carbon rod furnace to obtain the microwave dielectric ceramic material with adjustable dielectric constant.
[0040] The microwave dielectric properties of the materials obtained in Examples 1-6 are shown in Table 1, and the X-ray diffraction patterns of the materials obtained are shown in Figure 1 .
[0041] Table 1 Microwave dielectric properties of microwave dielectric ceramic materials of Examples 1-6
[0042] serial number x <![CDATA[ε r ]]> Q×f / GHz <![CDATA[τ f / (ppm / ℃) ]]> Example 1 0.7 10.0 68149 -7.5 Example 2 0.6 12.1 57641 -2.6 Example 3 0.5 14.4 57010 1.1 Example 4 0.4 15.8 54924 4.2 Example 5 0.3 17.3 48326 5.8 Example 6 0.15 19.9 47704 10.0
[0043] It can be seen from Table 1 that as the x value decreases: the dielectric constant gradually increases; the Q×f value gradually decreases, but always maintains a high level; the frequency temperature coefficient changes little, both meeting the actual application requirements of ≤±10ppm / ℃.
[0044] Depend on Figure 1 It can be seen that the diffraction peaks of the three phases of Mg2SiO4, Mg2TiO4 and CaTiO3 were found in all 6 embodiments, but the diffraction peak of the MO additive was not found, which shows that the three phases designed by the present invention exist independently and play the expected effect according to the design scheme. At the same time, as the x value changes from 0.7 to 0.15, the diffraction peak intensity corresponding to the Mg2SiO4 with a lower dielectric constant gradually weakens, and the diffraction peak intensity corresponding to the Mg2TiO4 with a higher dielectric constant gradually becomes stronger. This is the reason why the dielectric constant of the material of the present invention gradually increases and is adjustable as the x value decreases. At the same time, because the frequency temperature coefficients of the two phases of Mg2SiO4 and Mg2TiO4, which increase and decrease, are similar, the material of the present invention does not affect the frequency temperature coefficient as the dielectric constant changes.
[0045] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0046] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A microwave dielectric ceramic material with adjustable dielectric constant, characterized in that: The composition expression of the microwave dielectric ceramic material is: xMg2SiO4-(1-x)Mg2TiO4-0.09CaTiO3-0.005MO, wherein: 0.15≤x≤0.7, and MO is an auxiliary agent.
2. The microwave dielectric ceramic material with adjustable dielectric constant according to claim 1, characterized in that: The Mg2SiO4 and Mg2TiO4 have different dielectric constants and similar frequency temperature coefficients.
3. The microwave dielectric ceramic material with adjustable dielectric constant according to claim 1, characterized in that: In the additive MO, M is one or more of Fe, Zn, Nb, Si and Mg.
4. The microwave dielectric ceramic material with adjustable dielectric constant according to claim 1, characterized in that: The dielectric constant of the microwave dielectric ceramic material is adjustable in the range of 10.0 to 19.9, and the Q×f value is 47704 to 68149 GHz; the frequency temperature coefficient τ f ≤±10ppm / ℃.
5. The microwave dielectric ceramic material with adjustable dielectric constant according to claim 1 or 4, characterized in that: The dielectric constant of the microwave dielectric ceramic material gradually increases as the x value decreases.
6. The method for preparing a microwave dielectric ceramic material with adjustable dielectric constant according to claim 1, characterized in that: The method first prepares pre-synthesized powder I (Mg2SiO4-Mg2TiO4 phase) and pre-synthesized powder II (0.09CaTiO3-0.005MO) respectively; then the pre-synthesized powder I and the pre-synthesized powder II are subjected to secondary batching to complete three-phase composite; finally, the microwave dielectric ceramic material with adjustable dielectric constant is obtained through ball milling and sintering.
7. The method for preparing a microwave dielectric ceramic material with adjustable dielectric constant according to claim 1, characterized in that: The method comprises the following steps: (1) Ingredients: magnesium oxide, silicon dioxide, titanium dioxide, calcium carbonate and MO additive are used as raw materials. First, magnesium oxide, silicon dioxide and titanium dioxide are weighed according to the molar ratio of Mg, Si and Ti in Mg2SiO4 and Mg2TiO4 in the microwave dielectric ceramic material composition expression, and mixed evenly to obtain a mixture I. Then, titanium dioxide, calcium carbonate and MO additive are weighed according to the molar ratio of Ca, Ti and MO in CaTiO3 and MO in the microwave dielectric ceramic material composition expression, and mixed evenly to obtain a mixture II. (2) Mixing: ball-milling and drying the mixed material I and the mixed material II obtained in step (1) to obtain dry powder material I and dry powder material II; (3) Pre-sintering: placing the dry powder I and the dry powder II obtained in step (2) in different alumina crucibles, respectively, and pre-sintering them in a carbon rod furnace to obtain pre-synthesized powder I and pre-synthesized powder II; (4) Secondary batching: weigh and mix the pre-synthesized powder I (x Mg2SiO4-(1-x)Mg2TiO4) and pre-synthesized powder II (0.09CaTiO3-0.005MO) obtained in step (3) according to the composition of the microwave dielectric ceramic material to obtain secondary raw material powder; (5) slurry preparation: the secondary raw material powder obtained in step (4) is ball-milled for 20 to 26 hours, with the ball-milling medium being zirconium balls and deionized water, to obtain a viscous slurry; (6) Molding: Adding a binder accounting for 5 to 20 wt% of the slurry to the slurry obtained in step (5), then spray granulation and pressing molding are carried out in sequence, and finally sintering molding is carried out in a carbon rod furnace to obtain the microwave dielectric ceramic material with adjustable dielectric constant.
8. The method for preparing a microwave dielectric ceramic material with adjustable dielectric constant according to claim 7, characterized in that: In step (2), during the ball milling process, the ball milling medium is zirconium balls and deionized water; after ball milling, the product is placed in an oven at 150° C. and dried for 12 hours.
9. The method for preparing a microwave dielectric ceramic material with adjustable dielectric constant according to claim 7, characterized in that: In step (3), the pre-burning temperature in the carbon rod furnace is 1000° C. to 1200° C., and the pre-burning time is 2 to 4 hours.
10. The method for preparing a microwave dielectric ceramic material with adjustable dielectric constant according to claim 7, characterized in that: In step (6), the sintering temperature in the carbon rod furnace is 1250° C. to 1300° C., and the sintering time is 3 hours.
Citation Information
Patent Citations
Composite microwave dielectric ceramic and preparation method thereof
CN110922184A
Ceramic material and preparation method thereof, and ceramic sintered body and preparation method thereof
CN114180949A
Dielectric porcelain composition and dielectric resonator using the composition
EP1460645A2