Composite material sintered body, bonded body, member for semiconductor manufacturing device, and method for manufacturing composite material sintered body

By using a composite material sintered body of silicon carbide, tungsten silicide and tungsten carbide, the problem of reduced density in the existing technology is solved, the same linear thermal expansion coefficient and high strength as aluminum nitride are achieved, and it is suitable for electrostatic chuck cooling plates , improving the durability and cooling efficiency of semiconductor manufacturing equipment.

CN118724595AActive Publication Date: 2024-10-01NGK INSULATORS LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410271730.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-11
Publication Date
2024-10-01
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

When the existing composite material sintered body achieves the same linear thermal expansion coefficient as aluminum nitride, its density is reduced and it cannot meet the high strength and efficient heat dissipation requirements of the electrostatic chuck cooling plate.

Method used

A composite material sintered body composed of silicon carbide, tungsten silicide and tungsten carbide is used to ensure that the silicon carbide content is between 14.4wt% and below 48.6wt%, the opening porosity is below 1%, and the silicon carbide crystal is covered with tungsten silicide or tungsten carbide particles, increasing the content of tungsten silicide to increase strength and density.

Benefits of technology

It achieves the same linear thermal expansion coefficient as aluminum nitride, ensuring a dense composite material sintered body that is not easily peeled off under hot and cold cycles, and improves the durability and cooling efficiency of components used in semiconductor manufacturing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724595A_ABST
    Figure CN118724595A_ABST
Patent Text Reader

Abstract

The invention relates to a composite material sintered body, a bonded body, a member for a semiconductor manufacturing device, and a method for manufacturing the composite material sintered body, and provides a compact composite material sintered body which is composed of a constituent phase different from that in the prior art and has a linear thermal expansion coefficient difference with aluminum nitride equal to or smaller than that in the prior art. The composite material sintered body is composed of silicon carbide, tungsten silicide, and tungsten carbide, contains 14.4 wt% or more and 48.6 wt% or less of silicon carbide, and has an open porosity of 1% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite material sintered body. Background Art

[0002] For the electrostatic chuck which is heated in the semiconductor process, a cooling plate is connected to dissipate heat. For example, a dense sintered body of a composite material formed of silicon carbide, titanium silicide, titanium silicon carbide and titanium carbide is known as a preferred constituent material of the cooling plate when the material of the electrostatic chuck is alumina (see, for example, Patent Document 1). This composite material sintered body has the characteristics of having a small difference in linear thermal expansion coefficient with alumina, being dense and having high strength.

[0003] In addition, a dense sintered body of a composite material composed of silicon carbide, titanium silicon carbide, and titanium carbide is also known as a preferred constituent material of a cooling plate when the material of an electrostatic chuck is aluminum nitride (see, for example, Patent Document 2). This composite sintered body has the characteristics of having a small difference in linear thermal expansion coefficient with aluminum nitride, being dense, and having high strength.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-198662

[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-208567 Summary of the invention

[0008] The linear thermal expansion coefficient of aluminum nitride at 40°C to 570°C is 5.1 ppm / K, while the preferred range of the linear thermal expansion coefficient of the composite material disclosed in Patent Document 2 at 40°C to 570°C is 5.4 ppm / K to 6.0 ppm / K. In the Ti-Si-C composite material sintered body disclosed in Patent Document 2, if the linear thermal expansion coefficient of 5.1 ppm / K is to be achieved, the amount of silicon carbide needs to be increased. In this case, there is a problem that the density of the composite material sintered body is reduced and it is not suitable for the cooling plate of the electrostatic chuck.

[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide a dense composite material sintered body which is composed of a different constituent phase from the conventional ones, has a linear thermal expansion coefficient difference with aluminum nitride which is equal to or smaller than the conventional ones.

[0010] In order to solve the above problems, a first scheme of the present invention is a composite material sintered body, characterized in that it is composed of silicon carbide, tungsten silicide, and tungsten carbide, contains 14.4wt% to 48.6wt% of silicon carbide, and has an open porosity of 1% or less.

[0011] A second embodiment of the present invention is based on the composite material sintered body involved in the first embodiment, characterized in that the difference between the thermal expansion coefficient of the composite material sintered body at 40°C to 550°C and the thermal expansion coefficient of aluminum nitride at 40°C to 550°C is less than 0.5 ppm / K.

[0012] A third aspect of the present invention is the composite material sintered body according to the second aspect, wherein the open porosity is 0.1% or less.

[0013] The fourth scheme of the present invention is based on the composite material sintered body involved in any one of the first to third schemes, characterized in that the surface of each crystalline particle of silicon carbide is covered by at least one of tungsten silicide or tungsten carbide, thereby existing crystalline particles of at least one of tungsten silicide or tungsten carbide in the gaps between the crystalline particles of silicon carbide.

[0014] A fifth aspect of the present invention is the composite material sintered body according to any one of the first to fourth aspects, wherein the content of tungsten silicide is greater than the content of silicon carbide.

[0015] A sixth aspect of the present invention is the composite material sintered body according to any one of the first to fifth aspects, wherein the sintered body has a four-point bending strength of 200 MPa or more.

[0016] A seventh aspect of the present invention is the composite material sintered body according to the sixth aspect, wherein the sintered body has a four-point bending strength of 350 MPa or more.

[0017] An eighth aspect of the present invention is the composite material sintered body according to any one of the first to seventh aspects, wherein the thermal conductivity is 90 W / m·K or more.

[0018] A ninth aspect of the present invention is a composite material sintered body according to any one of the first to eighth aspects, characterized in that the fracture toughness value is 6.0 MPa·m 1 / 2 ~8.8MPa·m 1 / 2 .

[0019] A tenth aspect of the present invention is the composite material sintered body according to any one of the first to ninth aspects, wherein the Young's modulus is 273 GPa to 594 GPa.

[0020] An eleventh aspect of the present invention is the composite material sintered body according to the tenth aspect, wherein the Young's modulus is 460 GPa to 594 GPa.

[0021] The twelfth embodiment of the present invention is a joint body formed by joining a first component and a second component, and the joint body is characterized in that the first component is formed by a composite material sintered body, which is composed of silicon carbide, tungsten silicide, and tungsten carbide, contains more than 14.4wt% and less than 48.6wt% of silicon carbide, and has an open porosity of less than 1%, and the second component is formed by aluminum nitride.

[0022] A thirteenth aspect of the present invention is the bonded body according to the twelfth aspect, wherein the difference between the thermal expansion coefficient of the first member at 40°C to 550°C and the thermal expansion coefficient of the second member at 40°C to 550°C is 0.5 ppm / K or less.

[0023] A fourteenth aspect of the present invention is the bonded body according to the thirteenth aspect, wherein the open porosity of the first member is 0.1% or less.

[0024] A fifteenth aspect of the present invention is the joined body according to any one of the twelfth to fourteenth aspects, wherein the first member and the second member are joined by metal.

[0025] The sixteenth embodiment of the present invention is a component for semiconductor manufacturing equipment, which comprises a joint body formed by joining a first component and a second component. The component for semiconductor manufacturing equipment is characterized in that the first component is a cooling component for cooling the second component, and is formed by a composite material sintered body, the composite material sintered body is composed of silicon carbide, tungsten silicide, and tungsten carbide, contains more than 14.4wt% and less than 48.6wt% of silicon carbide, and has an open porosity of less than 1%, and the second component is formed by aluminum nitride.

[0026] The seventeenth scheme of the present invention is based on the component for semiconductor manufacturing equipment involved in the sixteenth scheme, characterized in that the difference between the thermal expansion coefficient of the first component at 40°C to 550°C and the thermal expansion coefficient of the second component at 40°C to 550°C is less than 0.5 ppm / K.

[0027] An eighteenth aspect of the present invention is the semiconductor manufacturing equipment member according to the seventeenth aspect, wherein the open porosity of the first member is 0.1% or less.

[0028] A nineteenth aspect of the present invention is the semiconductor manufacturing equipment member according to any one of the sixteenth to seventeenth aspects, wherein the first member and the second member are formed by metal bonding.

[0029] The twentieth scheme of the present invention is a method for manufacturing a composite material sintered body, characterized in that it includes the following steps: a mixing step, in which SiC powder, WSi2 powder, and WC powder or W powder are mixed to obtain a powder mixture; a molding step, in which the powder mixture is molded into a specified shape to obtain a molded body; and a sintering step, in which the molded body is hot-pressed and sintered in an inert atmosphere, in which 5.7wt% to 27.7wt% of SiC powder, 12.5wt% to 55.3wt% of WSi2 powder, and 49.5wt% to 81.3wt% of WC powder or 17.0wt% to 55.7wt% of W powder are mixed in a weight ratio of 100wt%, and in the sintering step, the maximum temperature is set to 1700℃ to 1850℃, and the pressing pressure is set to 225kgf / cm 2 ~300kgf / cm 2 .

[0030] The twenty-first embodiment of the present invention is based on the method for manufacturing a sintered composite material body involved in the twentieth embodiment, and is characterized in that in the mixing process, 5.7wt% to 13.1wt% of SiC powder, 12.5wt% to 39.1wt% of WSi2 powder, and 49.5wt% to 81.3wt% of WC powder are mixed in a weight ratio totaling 100wt%.

[0031] Effects of the Invention

[0032] According to the first to eleventh, twentieth and twenty-first aspects of the present invention, a dense composite material sintered body which is unlikely to peel off even when bonded to aluminum nitride and used under a thermal cycle is obtained.

[0033] Furthermore, according to the twelfth to nineteenth aspects of the present invention, component separation is unlikely to occur even when the bonded body is used under a thermal cycle, and therefore the service life of a component for a semiconductor manufacturing apparatus including the bonded body can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is an example of a cross-sectional SEM image of a sintered composite material.

[0035] Figure 2 This is a graph showing the relationship between the content of silicon carbide and the open porosity in a composite material sintered body.

[0036] Figure 3 This is an example of a curve of temperature and pressure during hot pressing. DETAILED DESCRIPTION

[0037] <Composite material sintered body>

[0038] The composite material sintered body involved in the present embodiment is a composite material sintered body containing silicon carbide (SiC), tungsten silicide, and tungsten carbide (WC) as crystalline phases. In the composite material sintered body involved in the present embodiment, when the total weight ratio of these crystalline phases is set to 100wt%, it contains 14.4wt% or more and 48.6wt% or less of silicon carbide (SiC). Preferably, the content of tungsten silicide is greater than the content of silicon carbide. Specifically, the tungsten silicide is WSi2 and W5Si3.

[0039] The composite material sintered body according to the present embodiment contains SiC, tungsten silicide and tungsten carbide as crystalline phases, which is confirmed by X-ray diffraction measurement of powder obtained by pulverizing the sintered body. In addition, the content of each substance is a value (simple quantitative value) obtained based on the diffraction peak of the X-ray diffraction measurement curve.

[0040] The composite material sintered body according to the present embodiment is a dense material (dense composite material sintered body) having an open porosity of 1% or less. The open porosity is a value measured by the Archimedean method using pure water as a medium.

[0041] More specifically, in the composite material sintered body according to the present embodiment, the surface of each crystal grain of silicon carbide is covered with at least one of tungsten silicide and tungsten carbide. Accordingly, crystal grains of at least one of tungsten silicide and tungsten carbide exist in the gaps between the crystal grains of silicon carbide.

[0042] Figure 1 This is an example of a cross-sectional SEM image of the sintered composite material body according to the present embodiment. Figure 1 In the image, the images of the four crystalline phases of SiC, WSi2, WC, and W5Si3 are seen in the order of brightness from low to high (from dark to bright). More specifically, it is confirmed that the roughly black crystal particles of SiC are separated from each other and the crystal particles of WSi2, WC, and W5Si3 cover the surroundings of each crystal particle without gaps.

[0043] In a sintered body with a high content of silicon carbide and high-frequency dispersion of silicon carbide particles, many pores may be generated between the particles. However, in the case of the composite material sintered body involved in this embodiment, the surface of the silicon carbide particles is covered by particles of other crystalline phases, so that such pores are almost not formed. Accordingly, the composite material sintered body involved in this embodiment is dense and high-strength.

[0044] The composite material sintered body according to the present embodiment preferably has an open porosity of 0.1% or less. A composite material sintered body satisfying this open porosity has extremely excellent density and extremely high strength.

[0045] Figure 2 This is a graph showing the relationship between the content of silicon carbide and the open porosity in various composite material sintered bodies produced under different production conditions. Specifically, the conditions of the maximum temperature and pressing pressure during hot pressing described later are different. Figure 2 In FIG. 5 , the data are plotted against the highest temperature during hot pressing. Figure 2 The following trend was confirmed: the more silicon carbide content in the composite material sintered body, the greater the open porosity. In particular, it can be seen that: in the range of silicon carbide content being approximately 50wt% or less, by setting the production conditions well, a composite material sintered body with an open porosity of less than 1% can be produced. In addition, it can be seen that: in the range of silicon carbide content being approximately 30wt% or less, a composite material sintered body with an open porosity of less than 0.1% can also be produced. On the other hand, when the silicon carbide content exceeds 50wt%, it is difficult to obtain a composite material sintered body with a smaller open porosity, so it is not preferred.

[0046] The linear thermal expansion coefficient of the composite material sintered body according to the present embodiment is approximately the same as the linear thermal expansion coefficient of aluminum nitride (AlN). In addition, the linear thermal expansion coefficient is hereinafter referred to as simply the thermal expansion coefficient.

[0047] Specifically, the difference between the thermal expansion coefficient of the composite material sintered body at 40°C to 550°C and the average thermal expansion coefficient of aluminum nitride at 40°C to 550°C (5.1 ppm / K) is 0.5 ppm / K or less. Specifically, the thermal expansion coefficient of the composite material sintered body at 40°C to 550°C is 4.6 ppm / K to 5.6 ppm / K, preferably 4.8 to 5.3 ppm / K.

[0048] Furthermore, the composite material sintered body according to the present embodiment has excellent thermal conductivity, and its thermal conductivity is 90 W / m·K or more, and preferably 100 W / m·K or more.

[0049] The composite material sintered body according to the present embodiment is also excellent in strength. Specifically, the four-point bending strength is 200 MPa or more, preferably 350 MPa or more, and more preferably 420 MPa or more.

[0050] The fracture toughness value (K1c) of the composite material sintered body according to the present embodiment is 6.0 MPa·m 1 / 2 ~8.8MPa·m 1 / 2 , preferably 6.2MPa·m 1 / 2 ~8.8MPa·m 1 / 2 .

[0051] Furthermore, the Young's modulus of the sintered composite material body according to the present embodiment may be 273 GPa to 594 GPa, preferably 330 GPa to 594 GPa, and more preferably 460 GPa to 594 GPa.

[0052] <Joint body>

[0053] As described above, the composite material sintered body according to the present embodiment has a thermal expansion coefficient similar to that of aluminum nitride. Therefore, even when the joint body obtained by joining (e.g., metal joining) a component (first component) formed by the composite material sintered body according to the present embodiment to a component (second component) made of aluminum nitride is used under repeated cold and hot cycles of low and high temperatures, the two components are not easily peeled off.

[0054] The joint body can be applied to, for example, parts for semiconductor manufacturing equipment. For example, a cooling plate (first part) made of the composite material sintered body involved in this embodiment and an electrostatic chuck (second part) made of aluminum nitride are joined using a joining material mainly composed of aluminum or its alloy to obtain parts for semiconductor manufacturing equipment.

[0055] In this bonded body or semiconductor manufacturing apparatus member, the difference in linear thermal expansion coefficient between the first member and the second member is extremely small, so that the first member is unlikely to be separated from the second member even when used under a thermal cycle.

[0056] Furthermore, since the first member formed of the composite material sintered body according to the present embodiment has sufficiently high thermal conductivity, the heat of the second member formed of aluminum nitride can be efficiently dissipated, and the second member can be efficiently cooled.

[0057] Furthermore, the first member formed of the composite material sintered body according to the present embodiment has a sufficiently high density and can have a structure that allows the coolant to pass through the inside. In this case, the cooling efficiency of the second member is further improved.

[0058] Furthermore, the first component formed by the composite material sintered body according to this embodiment has a sufficiently high strength and can therefore fully withstand stresses generated during processing and bonding for manufacturing components for semiconductor manufacturing equipment, as well as stresses generated by temperature differences when the component is used as a completed component.

[0059] That is, by using the composite material sintered body according to the present embodiment as a cooling plate of an electrostatic chuck, the service life of the component for semiconductor manufacturing equipment can be improved.

[0060] <Method for producing a sintered composite material>

[0061] Next, the manufacturing method of the composite material sintered body involved in this embodiment is described. In this embodiment, in summary, the desired composite material sintered body is obtained in the following order, that is, raw material powders weighed in a specified weight ratio are mixed to obtain a mixed powder, the mixed powder thus obtained is molded into a specified shape, and the obtained molded body is hot-pressed and sintered.

[0062] As raw material powder, 5.7wt% to 27.7wt% SiC, 12.5wt% to 55.3wt% WSi2, 17.0wt% to 55.7wt% tungsten (W) or 49.5wt% to 81.3wt% WC are prepared based on a total weight ratio of 100wt%. Preferably, the weight ratio of SiC is 6.0wt% or more and 13.1wt% or less.

[0063] The particle size of the raw material powder of SiC is not particularly limited, and the average particle size is preferably 2 μm to 35 μm. In addition, only coarse particles (for example, an average particle size of 15 μm to 35 μm) or only fine particles (for example, an average particle size of 2 μm to 10 μm) may be used, or coarse particles and fine particles may be mixed and used.

[0064] It should be noted that when using SiC powder with an average particle size of less than 2 μm, if the SiC ratio in the mixed powder is relatively large, the surface area of ​​the SiC particles increases, so the sinterability decreases and it is difficult to obtain a dense sintered body. On the other hand, when using SiC powder with an average particle size of more than 35 μm, even if there is no problem with sinterability, it is possible that sufficient strength cannot be obtained.

[0065] As the mixing of raw material powders, dry mixing using a high-speed fluid mixer can be exemplified. For example, if the total weight of the raw material powders is about 300 g to 500 g, it is preferred to set the rotation speed of the stirring blade of the high-speed fluid mixer to about 1000 rpm to 1500 rpm and stir for 10 to 15 minutes.

[0066] Alternatively, wet mixing using a nylon pot and an iron core nylon ball with isopropyl alcohol as a solvent may be performed. In this case, the mixed slurry is dried at 110° C. for 16 hours in a nitrogen stream, for example, and then sieved to obtain a mixed powder.

[0067] The hot press sintering of the compact obtained by molding the mixed powder is performed in an inert atmosphere. Examples of the inert atmosphere include a vacuum atmosphere, a nitrogen atmosphere, and an argon atmosphere.

[0068] The pressure during hot pressing (pressing pressure) is preferably 225 kgf / cm 2 ~300kgf / cm 2, more preferably 250kgf / cm 2 ~300kgf / cm 2 If the pressure is less than 200kgf / cm 2 , the sintered body is not densified and the open porosity exceeds 1%, which is not ideal.

[0069] Regarding the temperature during hot pressing, the maximum temperature is preferably 1700° C. to 1850° C., and more preferably 1770° C. to 1830° C. It should be noted that if the maximum temperature is 1900° C. or higher, the material melts and a sintered body of a desired shape cannot be obtained, which is not ideal. On the other hand, if the maximum temperature is less than 1700° C., sintering does not proceed sufficiently, which is not ideal.

[0070] Regarding the specific pressure and temperature curve during hot pressing (hereinafter, hot pressing conditions), it can be appropriately set within the above-mentioned preferred range according to the composition of the powder mixture (the weight ratio of each raw material powder), the particle size of the raw material powder, the size and shape of the molded body, etc. It should be noted that there is a trend that the smaller the weight ratio of silicon carbide in the mixed powder, the easier it is to sinter, so the permissible range of hot pressing conditions that can achieve densification is relatively wide. In addition, there is a trend that the permissible range of hot pressing conditions that can achieve densification is relatively wide when coarse particles and fine particles are mixed compared to the case where only coarse particles of silicon carbide are used.

[0071] In addition, about the firing time, similarly, it can be appropriately set according to the hot pressing conditions, the size and shape of the molded body, etc. For example, when a disk-shaped molded body with a diameter of 50 mm and a thickness of about 15 mm is hot pressed and fired, it is preferred to set the holding time of the maximum temperature within the range of 4 hours to 8 hours.

[0072] <Method for producing a bonded body>

[0073] A method (joining method) for obtaining a joined body formed by joining a first component formed by a composite material sintered body according to the present embodiment and a second component made of aluminum nitride is described. The joining method includes two types: metal joining in which two components are joined via a metal joining layer and direct joining in which two components are directly joined.

[0074] In the case of metal bonding, an aluminum metal foil and a dense aluminum nitride sintered body are sequentially stacked in this order on a composite material sintered body according to the present embodiment processed into a predetermined shape such as a disk, to obtain a stacked body, which is placed in a graphite mold for firing and hot-pressed in an inert gas atmosphere. Examples of the inert atmosphere include a vacuum atmosphere, a nitrogen atmosphere, an argon atmosphere, and the like.

[0075] The thickness of the metal foil may be about 180 μm to 220 μm. In addition, the stacking surfaces of the composite material sintered body, the metal foil, and the aluminum nitride are preferably of the same shape.

[0076] For hot pressing, the maximum temperature was set to 1770°C to 1830°C, and the pressing pressure was set to 250 kgf / cm 2 ~300kgf / cm 2 The value in this range can be obtained by setting the holding time at the maximum temperature to 4 to 8 hours. In this way, a bonded body (metal bonded body) having no interface peeling or voids can be obtained.

[0077] In the case of direct bonding, first, a powder mixture having a composition ratio that can obtain the composite material sintered body involved in this embodiment is subjected to uniaxial press molding under a predetermined pressurizing condition, thereby obtaining, for example, a disc-shaped molded body. Next, a dense aluminum nitride sintered body is stacked on the molded body to obtain a stacked body, which is placed in a graphite mold for firing and hot-pressed in an inert gas atmosphere. Examples of the inert atmosphere include: a vacuum atmosphere, a nitrogen atmosphere, an argon atmosphere, and the like.

[0078] In this case, the laminated surfaces of the molded body and the aluminum nitride are preferably of the same shape.

[0079] For hot pressing, the maximum temperature was set to 1770°C to 1830°C, and the pressing pressure was set to 250 kgf / cm 2 ~300kgf / cm 2 The value in this range can be obtained by setting the holding time of the maximum temperature to 4 to 8 hours. In this way, a bonded body (direct bonded body) having no peeling or voids at the interface can be obtained.

[0080] Example

[0081] The preparation and evaluation of composite material sintered bodies were attempted in 26 experimental examples with different combinations of raw material powder composition and hot pressing conditions. It should be noted that, hereinafter, the powder mixture, molded body, and sintered body of the same experimental example are sometimes not distinguished in their states and are collectively referred to as samples.

[0082] <Raw material powder>

[0083] As raw material powders, SiC, WSi2, W, and WC were prepared.

[0084] As raw material powders of SiC, three commercial products with different particle sizes were prepared. Specifically, three types of powders with average particle sizes of 36 μm (hereinafter referred to as #500 product), 15 μm (hereinafter referred to as #1000 product), and 3 μm (hereinafter referred to as #6000 product) were prepared. The purity of all of them was above 99%.

[0085] In addition, as the raw material powder of WSi2, a commercial product with a purity of 99% or more and an average particle size of 6 μm was used. As the raw material powder of WC, a commercial product with a purity of 99% or more and an average particle size of 2 μm was used. As the raw material powder of W, a commercial product with a purity of 99% or more and an average particle size of 2.3 μm was used.

[0086] <Production of sintered body>

[0087] The raw material compositions and hot pressing conditions of all the experimental examples are listed in Table 1. Table 1 also shows whether or not the samples melted during hot pressing.

[0088] Table 1

[0089]

[0090] In all experimental examples, when preparing the composite material sintered body, first, 300 g of SiC raw material powder, WSi2 raw material powder, and WC raw material powder or W raw material powder were weighed in total according to the composition ratio (weight ratio) shown in Table 1. The weighed three kinds of powders were placed in a high-speed flow mixer with a capacity of 1.8 L in the powder placement part, and stirred and mixed at 1500 rpm for 10 minutes to obtain a powder mixture.

[0091] The obtained powder mixture of each experimental example was subjected to a pressure of 200 kgf / cm 2 The uniaxial press molding was performed at a pressure of 1000 to produce a disk-shaped molded body with a diameter of 50 mm and a thickness of about 15 mm. The produced molded body was placed in a graphite mold for firing.

[0092] Then, the molded body is subjected to hot pressing to obtain a composite material sintered body. During the hot pressing, the maximum temperature is set to different levels, specifically 1650°C, 1700°C, 1770°C, 1800°C, 1830°C, 1850°C, and 1900°C. The holding time at the maximum temperature is set to 4 hours. In addition, the pressure is set to different levels, specifically 200kgf / cm 2 、225kgf / cm 2 、250kgf / cm 2 and 300kgf / cm 2 It should be noted that the pressure is applied when the sintering temperature reaches 900°C. Figure 3 The maximum temperature during hot pressing is 1800°C and the pressure is 250 kgf / cm 2 Example of a curve of temperature and pressure at .

[0093] <Composition and properties of sintered composite materials>

[0094] The constituent phases of the composite material sintered bodies obtained in each experimental example were identified and their composition ratios (contents) were calculated (simple quantification). In addition, the open porosity, bulk density, flexural strength, and thermal expansion coefficient were measured to evaluate the properties.

[0095] Table 2 lists the composition ratios of the constituent phases of the sintered bodies of the respective experimental examples, and the measurement results of the open porosity, bulk density, flexural strength, thermal expansion coefficient, fracture toughness value, Young's modulus, and thermal conductivity.

[0096] Table 2

[0097]

[0098] As shown in Table 2, Experimental Examples 1, 3 to 8, 10 to 12, 14 to 15, 17 to 19, and 21 to 25 correspond to Examples, and the other Experimental Examples correspond to Comparative Examples.

[0099] The fracture toughness value (K1c value), Young's modulus and thermal conductivity of some of the composite material sintered bodies of the examples were also measured. These measurement results are also shown in Table 2.

[0100] On the other hand, regarding Experimental Examples 16 and 20 in which the maximum temperature during hot pressing was set to 1900°C, as shown in Table 1, the sample melted during the firing process and a sintered body of the desired shape could not be obtained. Therefore, it was impossible to determine the constituent phases and measure any of the above-mentioned properties.

[0101] (Identification and simple quantification of constituent phases)

[0102] Except for Experimental Examples 16 and 20, the composite material sintered body obtained in the above order was crushed using a mortar and subjected to X-ray diffraction measurement (θ-2θ measurement) using a sealed tube X-ray diffractometer (D8 ADVANCE manufactured by Bruker AXS). Based on the peak pattern appearing in the obtained X-ray diffraction curve, the constituent phase (crystalline phase) of the composite material sintered body was identified. As characteristic X-rays, CuKα rays were used, the tube output was 40 kV, 40 mA, and the measurement range was 2θ = 5° to 70°.

[0103] In addition, the composition ratio (content) of the crystalline phase contained in the composite material sintered body was obtained by simple quantitative analysis based on the intensity of the peaks appearing in the X-ray diffraction curve. Simple quantitative analysis used the simple curve fitting function (FPM Eval.) of the powder diffraction data analysis software "EVA" of Bruker AXS. This function uses the I / Icor (intensity ratio relative to the corundum diffraction intensity) of the ICDD PDF card of the identified crystalline phase to calculate the weight ratio of the constituent phase.

[0104] (Determination of open porosity and bulk density)

[0105] The measurement was performed using the Archimedean method with pure water as the medium.

[0106] (Measurement of 4-point bending strength)

[0107] The measurement was conducted in accordance with JIS-R1601.

[0108] (Determination of thermal expansion coefficient)

[0109] The average linear thermal expansion coefficient at 40°C to 550°C was calculated using TD5020S (lateral differential expansion measurement method) manufactured by Bruker AXS Co., Ltd.

[0110] Specifically, the temperature was raised to 650°C twice at a heating rate of 20°C / min in an argon atmosphere, and the average linear thermal expansion coefficient was calculated based on the second measurement data. The standard sample used was an alumina standard sample (purity 99.7%, bulk density 3.9 g / cm 3 , length 20mm).

[0111] (Determination of fracture toughness value)

[0112] The fracture toughness was evaluated by the SEPB method in accordance with JIS-R1607.

[0113] (Determination of Young's modulus)

[0114] The Young's modulus is measured in accordance with JIS R1602 (Test method for elastic modulus of fine ceramics).

[0115] (Measurement of thermal conductivity)

[0116] The measurement was carried out using the laser flash method.

[0117] <Details of each experimental example>

[0118] (Experimental Example 1 to Experimental Example 5)

[0119] In Experimental Examples 1 to 5, a composite material sintered body was produced using powders of SiC, WSi2, and W as raw materials. As SiC powder, #500 and #6000 were used.

[0120] The raw material compositions are shown in Table 1, and in Experimental Examples 1 and 2, they are as follows.

[0121] SiC (#500): 18.0wt%;

[0122] SiC (#6000): 9.7wt%;

[0123] WSi2: 55.3wt%;

[0124] W: 17.0wt%.

[0125] Experimental Examples 3 to 5 are all as follows.

[0126] SiC (#500): 15.8wt%;

[0127] SiC (#6000): 8.5wt%;

[0128] WSi2: 20.0wt%;

[0129] W: 55.7wt%.

[0130] That is, in Experimental Examples 3 to 5, compared with Experimental Examples 1 and 2, the ratio of W was significantly increased, the ratio of WSi 2 was significantly reduced, and SiC was slightly reduced.

[0131] As hot pressing conditions, the maximum temperature was 1700°C in Experimental Examples 2 and 4, and the maximum temperature was 1800°C in Experimental Examples 1, 3, and 5. The pressing pressure was 250 kgf / cm 2 .

[0132] In Experimental Examples 1 to 5, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. The content of SiC in the sintered bodies was 48.6 wt % or less.

[0133] Among them, the open porosity of the sintered bodies of Experimental Examples 1 and Experimental Examples 3 to 5 was less than 1%, but the open porosity of the sintered body of Experimental Example 2 greatly exceeded 1%. That is, dense composite material sintered bodies were obtained in Experimental Examples 1 and Experimental Examples 3 to 5, but a dense composite material sintered body could not be obtained in Experimental Example 2.

[0134] More specifically, in Experimental Examples 1, 3, and 5, in which the maximum temperature during hot pressing was set to 1800°C, the open porosity was 1% or less. In contrast, in Experimental Examples 2 and 4, in which the maximum temperature during hot pressing was set to 1700°C, only the latter had an open porosity of 1% or less. The difference between Experimental Examples 2 and 4 is only the raw material composition, so it can be said that when W is used as the raw material, it is necessary to set the maximum temperature during hot pressing at least according to the raw material composition.

[0135] It should be noted that, except for Experimental Example 2, the thermal expansion coefficient was within the range of 4.6 ppm / K to 5.6 ppm / K. On the other hand, the bending strength exceeded 200 MPa but was less than 350 MPa in all Experimental Examples. In addition, in Experimental Examples 1, 4, and 5, the fracture toughness value (K1c) was 6.0 MPa·m 1 / 2 ~6.5MPa·m 1 / 2 , Young's modulus is 448 GPa to 484 GPa, and thermal conductivity is 100 W / m·K or more.

[0136] The results of Experimental Examples 1 to 5 show that when the weight ratio of SiC in the raw material powder is set to a value in the range of 5.7wt% to 27.7wt%, the weight ratio of WSi2 is set to a value in the range of 12.5wt% to 55.3wt%, and the weight ratio of W is set to a value in the range of 17.0wt% to 55.7wt%, and by appropriately setting the hot pressing conditions according to the raw material composition, a composite material sintered body is obtained, which contains silicon carbide of more than 14.4wt% and less than 48.6wt%, a dense material with an open porosity of less than 1%, and a thermal expansion coefficient close to that of aluminum nitride.

[0137] (Experimental Example 6 to Experimental Example 14)

[0138] In Experimental Examples 6 to 14, SiC, WSi2, and WC powders were used as raw materials to produce composite material sintered bodies. As SiC powder, only #1000 was used.

[0139] The raw material compositions are shown in Table 1, and in Experimental Examples 6 to 9, they are all as follows.

[0140] SiC (#1000): 13.1wt%;

[0141] WSi2: 22.2wt%;

[0142] WC: 64.7wt%.

[0143] In Experimental Example 10, the following is performed.

[0144] SiC (#1000): 11.4wt%;

[0145] WSi2: 39.1wt%;

[0146] WC: 49.5wt%.

[0147] Experimental Examples 11 to 13 are all as follows.

[0148] SiC (#1000): 9.1wt%;

[0149] WSi2: 31.5wt%;

[0150] WC: 59.4wt%.

[0151] In Experimental Example 14, it is as follows.

[0152] SiC (#1000): 8.5wt%;

[0153] WSi2: 19.6wt%;

[0154] WC: 71.9wt%.

[0155] That is, in Experimental Examples 6 to 9, Experimental Example 10, Experimental Example 11 to 13, and Experimental Example 14, the following relationship exists in this order: the weight ratio of SiC and WSi2 in the raw material decreases successively, and the weight ratio of WC increases successively.

[0156] On the other hand, as the hot pressing conditions, the maximum temperature was set to 1770°C in Experiment 7, 1830°C in Experiment 8, and 1800°C in all other experiments. In addition, the pressing pressure was 200 kgf / cm2 in Experiment 9 and Experiment 13. 2 , in addition, set to 250kgf / cm 2 .

[0157] That is, only the maximum temperature during hot pressing and firing differs in Experimental Examples 6 to 8. In addition, only the pressure during hot pressing and firing differs in Experimental Examples 6 and 9. Similarly, only the pressure during hot pressing and firing differs in Experimental Examples 11, 12, and 13.

[0158] On the other hand, regarding Experimental Examples 6, 10, 11, 12, and 14, the hot pressing conditions were the same, and only the raw material compositions were different.

[0159] The raw material composition and hot pressing conditions of Experimental Example 11 and Experimental Example 12 are the same.

[0160] In Experimental Examples 6 to 14, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. The SiC content in the sintered bodies was within a range of 14.4 wt% to 48.6 wt% in all Experimental Examples.

[0161] The pressing pressure during hot pressing was set to 200 kgf / cm 2 In Experimental Examples 9 and 13, the open porosity greatly exceeded 1%. That is, a dense composite material sintered body could not be obtained. On the other hand, the pressing pressure was set to 250 kgf / cm 2 In Experimental Examples 6 to 8, Experimental Examples 10 to 12, and Experimental Example 14, the open porosity was 0.1% or less. That is, a composite material sintered body of extremely excellent density was obtained.

[0162] It should be noted that in Experimental Examples 6 to 8, Experimental Examples 10 to 12 and Experimental Example 14, which obtained dense composite material sintered bodies, except for Experimental Example 7, the content of tungsten silicide (WSi2 and W5Si3) was greater than the content of silicon carbide (SiC).

[0163] The thermal expansion coefficient was within the range of 4.6 ppm / K to 5.6 ppm / K and within the range of 4.9 ppm / K to 5.3 ppm / K in all experimental examples. That is, the difference in thermal expansion coefficient from aluminum nitride was 0.2 ppm / K or less.

[0164] In addition, the composite material sintered bodies of Experimental Examples 6 to 8, Experimental Examples 10 to 12, and Experimental Example 14, which were judged to have extremely excellent dense properties with an open porosity of 0.1% or less, had a bending strength exceeding 350 MPa. In addition, the fracture toughness value (K1c) of these composite material sintered bodies was 6.3 MPa·m 1 / 2 ~7.9MPa·m 1 / 2 The Young's modulus was 448 GPa to 520 GPa except for Experimental Example 12 which was not measured. The thermal conductivity was 98 W / m·K in Experimental Example 11 and was 100 W / m·K or more in the other examples.

[0165] (Experimental Example 15 to Experimental Example 21)

[0166] In Experimental Examples 15 to 21, SiC, WSi2 and WC powders were used as raw materials to produce composite material sintered bodies. As SiC powder, #500 and #6000 were used in Experimental Examples 15 to 17, and only #1000 was used in Experimental Examples 18 to 21.

[0167] The raw material compositions are shown in Table 1, and in Experimental Examples 15 to 17, they are all as follows.

[0168] SiC (#500): 5.0wt%;

[0169] SiC (#6000): 1.2wt%;

[0170] WSi2: 12.5wt%;

[0171] WC: 81.3wt%.

[0172] In addition, in Experimental Examples 18 to 21, the following is true.

[0173] SiC (#1000): 6.2wt%;

[0174] WSi2: 12.5wt%;

[0175] WC: 81.3wt%.

[0176] That is, in Experimental Examples 15 to 21, the weight ratio of SiC and WSi2 was reduced, and the weight ratio of WC was increased, compared with Experimental Examples 6 to 14. In addition, in Experimental Examples 15 to 17 and Experimental Examples 18 to 21, the weight ratio of SiC as a whole was the same, and the particle size of the powder used was different.

[0177] On the other hand, as the hot pressing conditions, the maximum temperature was set to 1800°C in Experimental Examples 15 and 18, the maximum temperature was set to 1900°C in Experimental Examples 16 and 20, and the maximum temperature was set to 1830°C in Experimental Examples 17, 19, and 21. In addition, the pressing pressure was 250 kgf / cm 2 .

[0178] Results: As described above, in Experimental Examples 16 and 20 in which the maximum temperature during hot press sintering was set to 1900° C., the sample melted during sintering and a sintered body could not be obtained.

[0179] In Experimental Examples 15, 17 to 19, and 21, in which the highest temperature during hot pressing was 1800°C or 1830°C, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. In addition, the content of SiC in the sintered bodies was a value within the range of 14.4 wt% or more and 48.6 wt% or less in all the experimental examples.

[0180] In Experimental Examples 15, 17 to 19, and 21, the open porosity of the sintered bodies was 0.1% or less. That is, a composite material sintered body of extremely excellent density was obtained.

[0181] Furthermore, the thermal expansion coefficients of these sintered bodies were all within the range of 4.6 ppm / K to 5.6 ppm / K, that is, values ​​of 4.8 ppm / K to 4.9 ppm / K. That is, values ​​slightly smaller than the thermal expansion coefficient of aluminum nitride were obtained.

[0182] It should be noted that in Experimental Examples 15, 17 to 19, and 21, which obtained dense composite material sintered bodies, the content of tungsten silicide (WSi2 and W5Si3) was greater than the content of silicon carbide (SiC).

[0183] In addition, the composite material sintered bodies of Experimental Examples 15, 17 to 19, and 21, which were judged to be extremely excellent in density, had a bending strength exceeding 350 MPa. Furthermore, the fracture toughness value (K1c) of these composite material sintered bodies was 7.5 MPa·m 1 / 2 ~8.5MPa·m 1 / 2 , Young's modulus is 523 GPa to 561 GPa. These values ​​are generally higher than those in Experimental Examples 6 to 14. In addition, the thermal conductivity is 134 W / m·K or more, which is higher than that in Experimental Examples 6 to 14.

[0184] (Experimental Example 22 to Experimental Example 23)

[0185] In Experimental Examples 22 and 23, SiC, WSi2, and WC powders were used as raw materials to produce composite material sintered bodies. As SiC powder, only #1000 was used.

[0186] Regarding the raw material composition, as shown in Table 1, Experimental Example 22 is as follows.

[0187] SiC (#1000): 12.8wt%;

[0188] WSi2: 13.5wt%;

[0189] WC: 73.7wt%.

[0190] In addition, Experimental Example 23 is as follows.

[0191] SiC (#1000): 5.7wt%;

[0192] WSi2: 26.7wt%;

[0193] WC: 67.6wt%.

[0194] On the other hand, regarding the hot pressing conditions, the maximum temperature was 1800°C and the pressing pressure was 250 kgf / cm 2 .

[0195] That is, compared with Experimental Examples 6, 10, 11, 12, 14, and 18, which have the same hot pressing conditions, Experimental Examples 22 and 23 have different combinations of weight ratios of SiC powder (#1000 product), WSi2 powder, and WC powder as raw materials.

[0196] Sintered bodies were obtained in all experimental examples, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. The content of SiC in the sintered bodies was within the range of 14.4 wt% to 48.6 wt% in all experimental examples.

[0197] Among them, in Experimental Example 23, the content of tungsten silicide (WSi2 and W5Si3) is greater than the content of silicon carbide (SiC), but in Experimental Example 22, the opposite is true.

[0198] The open porosity of the sintered body was 0.1% or less in both Experimental Examples 22 and 23. That is, in all the Experimental Examples, a composite material sintered body of extremely excellent density was obtained.

[0199] On the other hand, the thermal expansion coefficient of the sintered body satisfies the range of 4.6 ppm / K to 5.6 ppm / K in all experimental examples, and in Experimental Example 22, it is the lower limit of the range, 4.6 ppm / K.

[0200] In Experimental Example 23, it was the upper limit of the range, 5.6 ppm / K.

[0201] In addition, regarding the bending strength, it was 423 MPa in Experimental Example 22, and it was 424 MPa in Experimental Example 23. That is, in all the experimental examples, it exceeded 350 MPa, but there was almost no difference between the two.

[0202] On the other hand, the fracture toughness value (K1c), Young's modulus, and thermal conductivity in Experimental Example 23 were 8.2 MPa·m 1 / 2 , 548 GPa, and 134 W / m·K, but in Experimental Example 22, they were limited to 6.0 MPa·m 1 / 2 , 332GPa, and 104W / m·K.

[0203] According to the comparison with other experimental examples, for Experimental Example 22, it is believed that the content of tungsten silicide (WSi2 and W5Si3) is 12.7wt% and is less than the content of silicon carbide (SiC) 28.1wt%, which may affect the characteristics of the sintered body. In addition, for Experimental Example 23, it is believed that the weight ratio of SiC in the raw material powder is as low as 5.7wt%, which may affect the characteristics of the sintered body.

[0204] (Experimental Example 24 to Experimental Example 26)

[0205] In Experimental Examples 24 to 26, a composite material sintered body was produced using powders of SiC, WSi2, and W as raw materials. As SiC powder, #500 and #6000 were used.

[0206] The raw material composition is shown in Table 1 and is the same as that of Experimental Examples 1 and 2, as follows.

[0207] SiC (#500): 18.0wt%;

[0208] SiC (#6000): 9.7wt%;

[0209] WSi2: 55.3wt%;

[0210] W: 17.0wt%.

[0211] As hot pressing conditions, in Experimental Examples 24 to 26, the combinations of maximum temperature and pressing pressure were different from those in Experimental Examples 1 to 5. In Experimental Example 24, the maximum temperature was set to 1850°C and the pressing pressure was set to 225 kgf / cm 2 In Experimental Example 25, the maximum temperature was set to 1700°C and the pressing pressure was set to 300 kgf / cm 2 In Experimental Example 26, the maximum temperature was set to 1650°C and the pressing pressure was set to 300 kgf / cm 2 .

[0212] That is, in Experimental Example 24, the maximum temperature was increased and the pressing pressure was decreased compared with Experimental Example 1. In Experimental Example 25, the pressing pressure was increased compared with Experimental Example 2 as a comparative example. In Experimental Example 26, the maximum temperature was decreased and the pressing pressure was increased compared with Experimental Example 2 as a comparative example.

[0213] In Experimental Examples 24 to 26, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. The content of SiC in the sintered bodies was less than 48.6 wt % in Experimental Examples 24 and 25, but was 50.1 wt % in Experimental Example 26, exceeding 48.6 wt %.

[0214] The open porosity of the sintered body was less than 1% in Experimental Examples 24 and 25, but exceeded 1% in Experimental Example 26.

[0215] In addition, the thermal expansion coefficient was 5.4 ppm / K, which satisfies the range of 4.6 ppm / K to 5.6 ppm / K, in all Experimental Examples 24 to 26. On the other hand, the bending strength was 252 MPa, which was similar to that of Experimental Examples 1 and 2, in Experimental Examples 24 and 25, but it was 116 MPa in Experimental Example 26. In addition, the fracture toughness values ​​(K1c) and Young's modulus of Experimental Examples 24 and 25 were similar to those of Experimental Example 1, but the thermal conductivity was slightly higher than that of Experimental Example 1.

[0216] (Summary of Experimental Examples 1 to 26)

[0217] The results of Experimental Examples 1 to 26 show that when the weight ratio of SiC in the raw material powder is set to a value in the range of 5.7wt% to 27.7wt%, the weight ratio of WSi2 is set to a value in the range of 12.5wt% to 55.3wt%, and the weight ratio of WC is set to a value in the range of 49.5wt% to 81.3wt% or the weight ratio of W is set to a value in the range of 17.0wt% to 55.7wt%, and by appropriately setting the hot pressing conditions, a composite material sintered body is obtained, which contains silicon carbide of more than 14.4wt% and less than 48.6wt%, a dense material with an open porosity of less than 1%, and a thermal expansion coefficient close to that of aluminum nitride.

[0218] In addition, it is also stated that the dense composite material sintered body has a 4-point bending strength of more than 200 MPa and a strength of 6.0 MPa·m 1 / 2 ~8.8MPa·m 1 / 2 The fracture toughness value is within this range, the Young's modulus is within the range of 273GPa to 594GPa, and the thermal conductivity is above 90W / m·K.

[0219] In particular, the results of Experimental Examples 6 to 23 also illustrate that when the weight ratio of SiC in the raw material powder is set to a value in the range of 5.7wt% to 13.1wt%, the weight ratio of WSi2 is set to a value in the range of 12.5wt% to 39.1wt%, and the weight ratio of WC is set to a value in the range of 49.5wt% to 81.3wt%, an extremely excellent dense composite sintered body with an open porosity of less than 0.1% is obtained, and the composite sintered body has an extremely excellent four-point bending strength of more than 350MPa.

Claims

1. A composite material sintered body, characterized in that: It is composed of silicon carbide, tungsten silicide, and tungsten carbide. Containing 14.4 wt% or more and 48.6 wt% or less of silicon carbide, The open porosity is 1% or less.

2. The composite material sintered body according to claim 1, characterized in that: The difference between the thermal expansion coefficient of the composite material sintered body at 40° C. to 550° C. and the thermal expansion coefficient of aluminum nitride at 40° C. to 550° C. is less than 0.5 ppm / K.

3. The composite material sintered body according to claim 2, characterized in that: The open porosity is 0.1% or less.

4. The composite material sintered body according to any one of claims 1 to 3, characterized in that: The surface of each crystal grain of silicon carbide is covered with at least one of tungsten silicide and tungsten carbide, so that crystal grains of at least one of tungsten silicide and tungsten carbide exist in gaps between crystal grains of silicon carbide.

5. The composite material sintered body according to any one of claims 1 to 3, characterized in that: The content of tungsten silicide is greater than that of silicon carbide.

6. The composite material sintered body according to any one of claims 1 to 3, characterized in that: The 4-point bending strength is 200 MPa or more.

7. The composite material sintered body according to claim 6, characterized in that: The 4-point bending strength is 350 MPa or more.

8. The composite material sintered body according to any one of claims 1 to 3, characterized in that: The thermal conductivity is above 90 W / m·K.

9. The composite material sintered body according to any one of claims 1 to 3, characterized in that: The fracture toughness value is 6.0MPa·m 1 / 2 ~8.8MPa·m 1 / 2 .

10. The composite material sintered body according to any one of claims 1 to 3, characterized in that: Young's modulus is 273GPa~594GPa.

11. The composite material sintered body according to claim 10, characterized in that: Young's modulus is 460GPa~594GPa.

12. A joined body, which is formed by joining a first component and a second component, The conjugate is characterized in that The first component is formed of a composite material sintered body, The composite material sintered body is composed of silicon carbide, tungsten silicide and tungsten carbide, contains 14.4wt% or more and 48.6wt% or less of silicon carbide, and has an open porosity of 1% or less. The second member is formed of aluminum nitride.

13. The joint body according to claim 12, characterized in that: A difference between a thermal expansion coefficient of the first member at 40° C. to 550° C. and a thermal expansion coefficient of the second member at 40° C. to 550° C. is 0.5 ppm / K or less.

14. The joint body according to claim 13, characterized in that: The first member has an open porosity of 0.1% or less.

15. The joint body according to any one of claims 12 to 14, characterized in that: The first member and the second member are metal-bonded.

16. A component for semiconductor manufacturing equipment, comprising a bonded body formed by bonding a first component and a second component, The semiconductor manufacturing device component is characterized in that: The first component is a cooling component for cooling the second component, and is formed of a composite material sintered body. The composite material sintered body is composed of silicon carbide, tungsten silicide and tungsten carbide, contains 14.4wt% or more and 48.6wt% or less of silicon carbide, and has an open porosity of 1% or less. The second member is formed of aluminum nitride.

17. The semiconductor manufacturing device component according to claim 16, wherein: A difference between a thermal expansion coefficient of the first member at 40° C. to 550° C. and a thermal expansion coefficient of the second member at 40° C. to 550° C. is 0.5 ppm / K or less.

18. The semiconductor manufacturing device component according to claim 17, wherein: The first member has an open porosity of 0.1% or less.

19. The semiconductor manufacturing device component according to any one of claims 16 to 18, wherein: The first member and the second member are metal-bonded.

20. A method for producing a composite material sintered body, characterized in that: Including the following processes: A mixing step, in which SiC powder, WSi2 powder, and WC powder or W powder are mixed to obtain a powder mixture; a molding step in which the powder mixture is molded into a predetermined shape to obtain a molded body; as well as a sintering step, in which the molded body is sintered by hot pressing in an inert atmosphere, In the mixing step, 5.7 wt% to 27.7 wt% of SiC powder, 12.5 wt% to 55.3 wt% of WSi2 powder, and 49.5 wt% to 81.3 wt% of WC powder or 17.0 wt% to 55.7 wt% of W powder are mixed in a weight ratio totaling 100 wt%. In the sintering process, the maximum temperature is set to 1700°C to 1850°C, and the pressing pressure is set to 225 kgf / cm 2 ~300kgf / cm 2 .

21. The method for producing a composite material sintered body according to claim 20, characterized in that: In the mixing step, 5.7 wt% to 13.1 wt% of SiC powder, 12.5 wt% to 39.1 wt% of WSi2 powder, and 49.5 wt% to 81.3 wt% of WC powder are mixed in a weight ratio totaling 100 wt%.

Citation Information

Patent Citations

  • Silicon carbide / tungsten carbide composite material and preparation method thereof

    CN101823882A

  • High-temperature preparation method of W-Si-C reactant

    CN107058840A

  • WC-SiC-BASED COMPOSITE WITH HIGH HARDNESS, HIGH YOUNG'S MODULUS AND HIGH FRACTURE TOUGHNESS VALUE, AND ITS MANUFACTURING METHOD

    JP2006089351A

  • WC-SiC-BASED COMPOSITE WITH HIGH HARDNESS, HIGH YOUNG'S MODULUS AND HIGH FRACTURE TOUGHNESS VALUE, AND ITS MANUFACTURING METHOD

    JP2010143822A