Aluminum nitride ceramic high-temperature annealing method

Through absolute ethanol and pure water cleaning, pickling, ultrasonic cleaning, multi-layer fixture protection and high-temperature annealing in a high-purity nitrogen protective atmosphere, the problem of surface particles and internal stress of aluminum nitride ceramics has been solved, achieving high cleanliness and Stability, suitable for semiconductor equipment.

CN118724613APending Publication Date: 2024-10-01HANGZHOU DAHE NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410913334.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Microscopic particles and residual stress are easily generated on the surface of aluminum nitride ceramics during high-temperature sintering and processing, which affects the cleanliness and stability of semiconductor equipment.

Method used

It adopts multi-layer protection design of absolute ethanol and pure water cleaning, HF-HNO3 pickling, ultrasonic cleaning, boron nitride fixture and aluminum nitride compact, combined with high-purity nitrogen protective atmosphere and high-temperature annealing method with precise temperature control. Thoroughly remove surface particles and reduce internal stress.

Benefits of technology

It achieves ultra-high cleanliness on the aluminum nitride ceramic surface and greatly reduces internal stress, improves the stability and service life of the product, and meets the requirements of semiconductor equipment for high cleanliness and high flatness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-temperature annealing method for aluminum nitride ceramic. The method comprises the following steps: S1, cleaning the surface of the aluminum nitride ceramic by using absolute ethyl alcohol and pure water; s2, the product is soaked in a mixed acid solution prepared from HF and HNO3 for surface acid pickling; s3, the product is placed in a solution formed by mixing pure water and absolute ethyl alcohol, and ultrasonic cleaning is conducted; s4, the cleaned aluminum nitride ceramic is placed in a boron nitride jig, and the boron nitride jig is placed in a vacuum sintering furnace; s5, annealing is started, the room temperature is increased to 600 DEG C, and the vacuum state is kept; s6, raising the temperature to 1500 DEG C from 600 DEG C, continuously introducing nitrogen, and keeping the temperature after the temperature rise is completed; and S7, the temperature is reduced to the room temperature, nitrogen is continuously introduced, and annealing is completed. According to the method, the internal stress accumulation of the ceramic is effectively eliminated by accurately controlling the heat treatment environment and process parameters, the dimensional stability and the use reliability of a final product are ensured, and the strict requirements of semiconductor manufacturing on high-performance materials are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum nitride ceramic processing, in particular to a high-temperature annealing method for aluminum nitride ceramic. Background Art

[0002] In the high-end semiconductor equipment manufacturing industry, aluminum nitride ceramics are widely used in thin film deposition equipment, photolithography machines, etc. chip processing equipment due to their excellent thermal conductivity. However, due to their high sintering temperature (greater than 1800°C) and their direct contact with wafers in actual work, and being subject to a certain extrusion pressure, their surface cleanliness and internal residual stress have a very large impact on the stable operation of semiconductor equipment.

[0003] On the one hand, aluminum nitride ceramic materials are very brittle, and a large number of microscopic aluminum nitride particles will be generated on the ceramic surface during the processing. If they are not cleaned up, these particles will contaminate the wafer when they come into direct contact with the wafer. On the other hand, aluminum nitride ceramics have large residual stress during sintering and processing. If it is not reduced, it will easily cause local cracking of the ceramic product during the operation of the semiconductor equipment.

[0004] For example, the "method for removing particles from the surface of ceramic products" disclosed in Chinese patent documents, with application number "CN2019113952871", includes the following steps: a. preparation before annealing; b. formal annealing: after the kiln car enters the furnace, select the annealing program and ignite it, the annealing program includes step b1, step b2 and step b3; b1: raise the temperature in the furnace to a maximum temperature of 1000-1005°C; b2: start cooling after keeping the highest temperature for 30-40 minutes; b3: the cooling rate is 10-20°C / hr, and keep at least one temperature in the range of 900°C-800°C for 30-40 minutes, and the cooling end temperature is 100-250°C; c. completion of annealing: take the ceramic parts out of the furnace.

[0005] From the result data of this scheme, it can be seen that the aluminum nitride ceramic product of the present invention has a significantly reduced number of surface particles compared to the aluminum nitride ceramic product made by the traditional process, thus improving the product quality. Therefore, the processing scheme needs to be further optimized. Summary of the invention

[0006] In view of the problem in the prior art that microscopic particles are easily left on the surface of aluminum nitride ceramic materials, the present invention provides a high-temperature annealing method for aluminum nitride ceramics, which can effectively and significantly reduce the number of surface microscopic particles and internal residual stress, thereby enabling it to be used stably in semiconductor equipment.

[0007] The second invention objective of the present invention is to solve the problem that aluminum nitride ceramics have large residual stress that is difficult to eliminate during sintering and processing.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions: A high temperature annealing method for aluminum nitride ceramics comprises the following steps: S1: Use anhydrous ethanol and pure water to clean the surface of aluminum nitride ceramics; S2: Immerse the product in a mixed acid solution prepared by HF and HNO3 for surface pickling; S3: placing the product in a solution of pure water and anhydrous ethanol for ultrasonic cleaning; S4: placing the cleaned aluminum nitride ceramic in a boron nitride fixture and placing it in a vacuum sintering furnace; S5: Annealing begins, the room temperature rises to 600°C, and the vacuum state is maintained; S6: Raise the temperature from 600°C to 1500°C, continue to introduce nitrogen, and keep warm after the temperature is raised; S7: Cool down to room temperature, continue to introduce nitrogen, and annealing is completed.

[0009] The method first uses S1-S3 multi-step cleaning, using anhydrous ethanol, pure water and mixed acid solution to thoroughly remove various pollutants and microscopic particles on the ceramic surface. Once these particles come into contact with the wafers to be processed later, they can easily cause product contamination and seriously affect the normal operation of semiconductor equipment. Therefore, achieving ultra-high surface cleanliness is the primary task of this method.

[0010] Next, in S4, the cleaned ceramic sample is placed in a special boron nitride fixture and fixed with an aluminum nitride block. This design not only creates an ideal high-temperature processing environment, which is conducive to subsequent precise control, but also can minimize the interference of external factors on the process and ensure the stability of the entire annealing process.

[0011] Finally, in the high temperature annealing stage of S5-S7, by strictly controlling the parameters such as heating and cooling rate, maximum temperature, and holding time, combined with nitrogen protective atmosphere, the stress accumulation inside the ceramic material is effectively eliminated. This precise heat treatment process can greatly reduce the residual stress level and avoid defects such as cracking in actual use, thereby greatly improving the stability of the product.

[0012] Compared with the common simple sintering process, this method has carried out targeted design optimization in key links such as cleaning, protection, and heat treatment, which not only solves the problem of surface particles, but also solves the problem of internal stress, reflecting strong innovation. This can not only meet the stringent requirements of high-end semiconductor equipment for high cleanliness and high flatness, but also provide a strong guarantee for the application of aluminum nitride ceramic materials in this field.

[0013] Preferably, in the mixed acid solution in S2, the HF concentration is 20%-30%, and the HNO3 concentration is 40%-50%.

[0014] The purpose of the pickling process is to further thoroughly remove all kinds of pollutants and microscopic particles on the surface of aluminum nitride ceramics. The aforementioned claim 1 has achieved preliminary surface purification through steps such as cleaning and ultrasound. Due to the characteristics of the aluminum nitride ceramic material itself, a large number of microscopic particles are easily generated on the surface during high-temperature sintering and processing. If they are not completely removed, they are very likely to contaminate subsequent wafers. By optimizing the proportion of the pickling solution components, the cleaning effect can be maximized. The synergistic effect of HF and HNO3 can effectively dissolve and remove various inorganic impurities remaining on the surface, including aluminum nitride microparticles. The concentrations of the two acids are controlled within the range of 20%-30% and 40%-50%, respectively, in order to seek the best balance between cleaning effect and material damage. Excessive acid concentration may cause surface corrosion and damage, affecting subsequent high-temperature annealing. Therefore, the parameter setting fully considers the controllability of the process and the coordination of product performance. Compared with conventional simple water washing or ultrasonic cleaning, the pickling process significantly improves the surface cleanliness and creates more ideal basic conditions for subsequent high-temperature annealing. This not only helps to further reduce surface microscopic particles, but also prevents these particles from contaminating key components during actual use, thereby effectively improving the stability and service life of the product in semiconductor equipment.

[0015] Preferably, the volume ratio of pure water to anhydrous ethanol in S1 and S3 is 1:1 to 3:1, the ultrasonic intensity is 10-20W / In2, and the frequency is 35-45kHz. In the surface cleaning process of S1, a mixed solution of pure water and anhydrous ethanol is used, and the volume ratio is 1:1 to 3:1. Such a solvent ratio design can ensure the best balance between cleaning effect and material damage. Pure water has excellent decontamination ability, while anhydrous ethanol can avoid residual water, thereby preventing oxidation reaction during subsequent high-temperature annealing. Through the proper combination of the two solvents, surface contamination can be removed to the maximum extent without causing damage to the ceramic substrate. Secondly, in the ultrasonic cleaning link of S3, the applicant set specific intensity and frequency parameters, which are 10-20W / In2 and 35-45kHz respectively. This optimized design is conducive to further improving the cleaning effect and ensuring the thorough removal of surface contaminants. Ultrasonic cleaning, as an efficient physical cleaning method, can effectively peel off microscopic particles, organic matter, etc. on the ceramic surface with a strong impact force. Precise control of the intensity and frequency of the ultrasound can maximize the cleaning effect while avoiding damage to the surface due to excessive erosion.

[0016] Preferably, the upper and lower sides of the boron nitride sintering jig described in S4 are provided with aluminum nitride ceramic jigs, and the aluminum nitride ceramic jig on the upper side of the boron nitride sintering jig is pressed and provided with an aluminum nitride pressing block. This multi-level protection design can effectively prevent the deformation of ceramics at high temperatures. The boron nitride jig can provide an ideal high-temperature processing environment for the sample, while the aluminum nitride jigs on both sides and the pressing block on the top play a role of clamping and fixing. This can not only prevent the sample from warping or deformation during the heating process, but also ensure that its surface maintains excellent flatness, creating favorable conditions for subsequent microstructure adjustment. Compared with conventional single jigs or open furnaces, this multiple protection design significantly improves the stability and controllability of the process. This is conducive to reducing the surface roughness of the product, reducing internal stress, ensuring that the entire high-temperature annealing process can proceed smoothly as expected, and obtaining ideal product performance.

[0017] Preferably, the surface roughness of the aluminum nitride ceramic fixture and the aluminum nitride block is Ra0.6-Ra0.4. This fine surface roughness requirement reflects the applicant's in-depth grasp of the details of the high-temperature process environment. During the high-temperature sintering process of aluminum nitride ceramics, the microscopic morphology of the fixture surface will directly affect the heat treatment effect of the sample. An overly rough surface may cause local deformation or adhesion of the ceramic when heated, affecting the overall dimensional stability. An overly smooth surface may cause sliding or detachment between the sample and the fixture, which also affects the controllability of the heat treatment process. By accurately controlling the surface roughness of the fixture within the range of Ra0.6-Ra0.4, the heat treatment environment is optimized. This detailed design is not only conducive to ensuring that the sample maintains good dimensional stability at high temperatures, but also creates more ideal prerequisites for subsequent high-temperature annealing processes. Compared with the conventional solution of using a natural fixture or simply roughening it, this precise roughness control reflects the applicant's in-depth understanding of material behavior and process requirements. This targeted optimization design can effectively improve the thermal conductivity between the fixture and the sample and reduce local stress concentration, thus laying the foundation for obtaining high-quality aluminum nitride ceramic products.

[0018] Preferably, the heating rate from room temperature to 600°C in S5 is 1-3°C / min; the heating rate from 600°C to the maximum temperature of 1300-1500°C is also 1-3°C / min. This precise temperature rise and fall control is crucial to ensure the controllability of the high temperature annealing process and product quality. Aluminum nitride ceramics, as a typical brittle material, are prone to microstructural evolution such as phase change and grain growth at high temperatures, resulting in internal stress accumulation. If the heating rate is too fast, these structural changes will not have time to balance, resulting in defects such as stress concentration and cracking. By setting a reasonable temperature rise and fall rate, i.e. 1-3°C / min, it can be ensured that the thermal stress during the heat treatment process is within a controllable range, so that the microstructural evolution can proceed smoothly. This fine parameter optimization is not only conducive to minimizing the internal stress level of ceramic products, but also can ensure its stability and reliability in subsequent use.

[0019] Preferably, the holding time at the highest temperature in S6 is 1-3 hours. This ultra-high purity nitrogen environment is conducive to minimizing the oxidation reaction of ceramics at high temperatures, thereby effectively reducing the generation of internal stress and defects. Compared with the conventional use of ordinary industrial-grade nitrogen, or the simple use of an open furnace, this ultra-high purity nitrogen protection significantly improves the controllability of the process. High-purity nitrogen can effectively isolate the influence of outside air and provide an ideal inert atmosphere for ceramic samples. This is not only conducive to inhibiting surface oxidation reactions, but also avoids the introduction of other impurities, ensuring the stability of the entire heat treatment process. From the perspective of process effects, the protective atmosphere design helps to further reduce the internal stress level of ceramic materials and enhance their service life in semiconductor equipment.

[0020] Preferably, in S6 and S7, during the heating and insulation process, the flow rate of nitrogen introduced into the furnace is 10 NL / min. Through precise time control, it not only helps to improve the energy efficiency of the process, but also ensures the appropriateness of the heat treatment. For brittle ceramic materials, heat treatment at high temperature for too long can easily lead to excessive grain growth, resulting in internal stress accumulation and crack defects. However, too short a time cannot fully adjust the microstructure and eliminate residual stress. Therefore, the applicant reasonably controls the entire high-temperature annealing process to be completed within 18-24 hours, which not only meets the sufficient heat treatment requirements, but also avoids the disadvantages of excessive heat treatment. This targeted time parameter optimization, combined with the aforementioned temperature rise and fall rate control, forms a highly optimized high-temperature process solution.

[0021] Preferably, the cooling rate described in S7 is 0.5-2°C / min. For brittle ceramic materials, the microstructure evolution and phase change behavior have a crucial impact on their final performance during the heat treatment process at high temperature. Therefore, it is necessary to ensure that these microscopic behaviors can proceed smoothly by reasonably controlling the temperature parameters, thereby minimizing the generation of internal stress and defects. Specifically, the 1400-1500°C heating in S5 can create ideal thermodynamic conditions for subsequent structural adjustments. The 2-4 hours of heat preservation in S6 is conducive to fully completing the processes such as grain growth and phase change, and eliminating internal stress accumulation. Finally, the 3-5°C / min slow cooling in S7 can avoid stress concentration during thermal shrinkage and ensure the dimensional stability and excellent performance of the final product. The method has carried out targeted temperature parameter design in each stage of heating, heat preservation and cooling. This step-by-step fine control is not only conducive to obtaining an ideal microstructure, but also creates a good foundation for subsequent performance.

[0022] Preferably, the surface flatness of the aluminum nitride ceramic product after annealing is Ra≤0.4 μm, and the internal residual stress is reduced to ≤20 MPa. Surface roughness and internal stress level are two key indicators for judging the applicability of ceramic materials in semiconductor devices. Too high roughness will affect the surface finish and micro-machining accuracy of the product, while too large internal stress can easily lead to defects such as cracking, seriously affecting the service life.

[0023] Therefore, the present invention has the following beneficial effects: (1) Achieve ultra-high cleanliness on the surface of aluminum nitride ceramics, completely remove microscopic particles and impurities, effectively prevent semiconductor equipment from being contaminated during use, and greatly improve the applicability of the product in this field. (2) By precisely controlling the heat treatment environment and process parameters, effectively eliminate the internal stress accumulation of ceramics, ensure the dimensional stability and reliability of the final product, and meet the strict requirements of semiconductor manufacturing for high-performance materials. (3) Targetedly optimize process details such as cleaning solvents, ultrasonic parameters, and fixture design, give full play to material properties and process laws, and improve the pertinence and practicality of the overall method. (4) Comprehensively apply a number of innovative designs, such as ultra-high purity nitrogen protection and step-by-step temperature control, to bring new solutions to the application of aluminum nitride ceramics in the semiconductor field. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with specific implementation methods.

[0025] Example 1 (1) Use 95% pure anhydrous ethanol to scrub the surface of the aluminum nitride ceramic sample, and then rinse it with pure water; (2) Use hydrofluoric acid and nitric acid to prepare a mixed acid solution in the ratio of HF:HNO3=1:1, place the product in it and soak for 20 minutes, take it out and rinse it with pure water; (3) Use pure water and anhydrous ethanol to prepare a mixed solution in the ratio of pure water: anhydrous ethanol=1:1, introduce the solution into an ultrasonic cleaning tank, set the ultrasonic intensity to 10W / In2, set the power to 35KHz, then place the product in the mixed solution for ultrasonic treatment, take it out after washing for 10 minutes, rinse it with pure water, place it in an oven for 30 minutes, and take it out after drying; (4) Place the product with the cleaned and dried surface in a boron nitride sintering fixture, and place the cleaned aluminum nitride ceramic fixtures on the upper and lower parts of it, and finally press it with an aluminum nitride block on the upper part, and then place it in a vacuum sintering furnace; (5) During the annealing process from room temperature to 600°C, the heating rate is controlled at 1°C / min, and the vacuum state is maintained in the furnace; (6) The maximum annealing temperature is set to 1300°C, and the heating rate from 600°C to 1300°C is controlled at 1°C / min. The maximum temperature holding time is 3h, and nitrogen gas must be continuously introduced into the furnace at a nitrogen flow rate of 10NL / min to ensure a nitrogen atmosphere in the furnace; (7) The cooling rate is controlled at 0.5°C / min, and nitrogen gas must be continuously introduced into the furnace during the cooling process at a nitrogen flow rate of 10NL / min to ensure a nitrogen atmosphere in the furnace. After the temperature drops to room temperature, the ceramic is taken out of the sintering vacuum furnace.

[0026] Example 2 (1) Use 95% pure anhydrous ethanol to scrub the surface of the aluminum nitride ceramic sample, and then rinse it with pure water; (2) Prepare a mixed acid solution using hydrofluoric acid and nitric acid in a ratio of HF:HNO3=1:2, soak the product in it for 30 minutes, and rinse it with pure water after taking it out; (3) Use pure water and anhydrous ethanol to prepare a mixed solution in a ratio of pure water: anhydrous ethanol = 2:1, introduce the solution into an ultrasonic cleaning tank, set the ultrasonic intensity to 15W / In2, and the power to 40KHz, then place the product in the mixed solution for ultrasonic treatment, take it out after washing for 20 minutes, rinse it with pure water, place it in an oven for 45 minutes, and take it out after drying; (4) Place the cleaned and dried product in a boron nitride sintering jig, and place cleaned aluminum nitride ceramic jigs on the top and bottom of the jig. Finally, press the top with an aluminum nitride press block, and then place it in a vacuum sintering furnace. (5) The heating rate of the annealing process from room temperature to 600°C is controlled at 2°C / min, and the furnace is kept in a vacuum state; (6) The maximum annealing temperature is set to 1400°C, and the heating rate from 600°C to 1400°C is controlled at 2°C / min. The maximum temperature holding time is 2h. Nitrogen gas needs to be continuously introduced into the furnace, and the nitrogen flow rate is 10NL / min to ensure the nitrogen atmosphere in the furnace. (7) The cooling rate is controlled at 1°C / min, and nitrogen needs to be continuously introduced into the furnace during the cooling process. The nitrogen flow rate is 10NL / min to ensure the nitrogen atmosphere in the furnace. After the temperature drops to room temperature, the ceramics are taken out of the sintering vacuum furnace.

[0027] Example 3 (1) Use 95% pure anhydrous ethanol to scrub the surface of the aluminum nitride ceramic sample, and then rinse it with pure water; (2) Prepare a mixed acid solution using hydrofluoric acid and nitric acid in a ratio of HF:HNO3=1:3, soak the product in it for 40 minutes, and rinse it with pure water after taking it out; (3) Use pure water and anhydrous ethanol to prepare a mixed solution in a ratio of pure water: anhydrous ethanol = 3:1, introduce the solution into an ultrasonic cleaning tank, set the ultrasonic intensity to 20W / In2, and the power to 45KHz, then place the product in the mixed solution for ultrasonic treatment, wash it for 30 minutes and then take it out, rinse it with pure water, place it in an oven for 1 hour, and take it out after drying; (4) Place the cleaned and dried product in a boron nitride sintering jig, and place cleaned aluminum nitride ceramic jigs on the top and bottom of the jig. Finally, press the top with an aluminum nitride press block, and then place it in a vacuum sintering furnace. (5) The heating rate of the annealing process from room temperature to 600°C is controlled at 3°C / min, and the furnace is kept in a vacuum state; (6) The maximum annealing temperature is set to 1500℃, and the heating rate from 600℃ to 1500℃ is controlled at 3℃ / min. The maximum temperature holding time is 1h. Nitrogen gas needs to be continuously introduced into the furnace, and the nitrogen flow rate is 10NL / min to ensure the nitrogen atmosphere in the furnace. (7) The cooling rate is controlled at 2°C / min, and nitrogen needs to be continuously introduced into the furnace during the cooling process. The nitrogen flow rate is 10NL / min to ensure the nitrogen atmosphere in the furnace. After the temperature drops to room temperature, the ceramics are taken out of the sintering vacuum furnace.

[0028] Comparative Example Use 95% pure anhydrous ethanol to scrub the surface of the aluminum nitride ceramic sample, and then rinse it with pure water.

[0029] Test Case The particle count test on the ceramic surface is carried out using a particle detector (the test area of ​​the ceramic sample surface is 100cm 2 ); The residual stress was tested using an X-ray stress meter; project 0.3~1μm particle number / piece 1~5μm particle number / piece 5~10μm particles / piece Residual stress / MPa Example 1 3754 278 2 27 Example 2 3563 229 1 18 Example 3 3626 246 3 35 Comparative Example 5566 463 13 113 From the results in the table above, it can be seen that the number of surface particles and residual stress of aluminum nitride ceramics after annealing using this method are greatly reduced, which has a significant effect.

[0030] Through the comparative analysis of the above embodiments, it can be clearly understood that the scheme of the present invention is intended to provide an optimized high-temperature annealing process for aluminum nitride ceramics to solve the key problems existing in the application of the prior art in this field. Aluminum nitride, as a typical high-performance ceramic material, is widely used in the manufacture of semiconductor equipment due to its excellent thermal conductivity, electrical insulation and corrosion resistance. However, during high-temperature sintering and processing, a large number of microscopic particles and impurities are often produced on its surface, which seriously affects the cleanliness and performance stability of subsequent wafers. At the same time, ceramics are also prone to deformation and internal stress accumulation during high-temperature heat treatment, further reducing the dimensional accuracy and service life of the product.

[0031] In response to the above problems, the applicant proposed an optimized high-temperature annealing process, including key steps such as surface cleaning, pickling, ultrasonic cleaning, and high-temperature annealing.

[0032] First, in the surface cleaning S1 stage, the applicant used a mixed solution of pure water and anhydrous ethanol. This solvent ratio design fully considers the balance between decontamination effect and material damage. The water solvent has excellent decontamination performance, while anhydrous ethanol can effectively avoid oxidation reactions during subsequent high-temperature treatment. Through the proper combination of the two solvents, surface contamination can be removed to the maximum extent without causing damage to the brittle ceramic substrate.

[0033] Then, in the pickling treatment of S2, the applicant used a mixed acid solution with an HF concentration of 20%-30% and an HNO3 concentration of 40%-50%. This pickling formula can effectively dissolve and remove various inorganic impurities remaining on the surface, including aluminum nitride microparticles produced during the sintering process. The synergistic effect of the acid and solvent is conducive to achieving a more thorough cleaning effect and creating high-quality basic conditions for subsequent high-temperature annealing.

[0034] In the ultrasonic cleaning process of S3, the applicant further improved the surface cleanliness by precisely controlling the power and frequency parameters. High-intensity ultrasonic oscillation can effectively remove microscopic particles and organic pollutants on the ceramic surface with strong impact force. The optimized design of ultrasonic treatment conditions can maximize the cleaning effect while avoiding unnecessary damage caused by excessive surface erosion.

[0035] For the process details of high temperature annealing S4-S7, the invention scheme also proposed innovative optimization measures. First, in the sintering fixture design of S4, in addition to the boron nitride liner, the applicant also added additional aluminum nitride ceramic fixtures on the upper and lower sides, and placed aluminum nitride blocks on the upper part. This multi-layer fixture protection can effectively prevent the ceramic from warping or deformation at high temperatures, creating ideal environmental conditions for subsequent microstructure adjustments.

[0036] In terms of specific temperature parameter control, the scheme also reflects the applicant's in-depth understanding of the laws of high-temperature processes. The precise heating (1-3°C / min to 1400-1500°C), heat preservation (1400-1500°C, 2-4 hours), and cooling (3-5°C / min) parameters set in S5-S7 ensure that the microstructure evolution and phase change process can proceed smoothly, minimizing the accumulation of internal stress. This step-by-step temperature control, combined with the aforementioned multi-layer fixture protection design, is conducive to obtaining ceramic products with stable dimensions and excellent performance.

[0037] In addition, the scheme has also made innovations in the design of protective atmosphere for high-temperature annealing. The applicant used high-purity nitrogen with a purity of more than 99.999%, which effectively isolated the influence of external air and provided an ideal inert atmosphere environment for ceramic samples. This kind of atmosphere protection can effectively inhibit the oxidation reaction on the surface and ensure that no other impurities are introduced during the microstructure adjustment process, thereby helping to further reduce the internal stress level.

[0038] Overall, the invention scheme gives full play to the synergistic optimization effect of each process link, effectively improves product performance and process stability, and brings new solutions for the application of aluminum nitride ceramics in the semiconductor field.

[0039] First, in the surface cleaning and pickling process, the applicant used a pure water-anhydrous ethanol mixed solution and a HF-HNO3 composite acid solution, which can effectively remove various inorganic particles and organic pollutants on the ceramic surface. This targeted cleaning process design creates an ideal clean foundation for the subsequent high-temperature annealing process. Compared with the traditional simple water washing or single pickling solution, this cleaning process can more thoroughly eliminate surface contamination and ensure that the product will not cause secondary contamination in semiconductor equipment.

[0040] In terms of high-temperature annealing process, by precisely controlling the time-temperature parameters of each stage such as heating, heat preservation, and cooling, the applicant ensured the controllability of the microstructure evolution process and minimized the accumulation of residual stress. At the same time, the multi-layer fixture protection design effectively prevented the ceramic from deforming at high temperatures, laying the foundation for obtaining dimensionally stable products. This systematic process optimization is crucial to improving product reliability and service life.

[0041] In addition, the solution has also made innovations in the control of protective atmosphere. The use of high-purity nitrogen with a purity of more than 99.999% effectively isolates the influence of external air on the ceramic microstructure and ensures the controllability of the heat treatment process. Compared with the simple use of ordinary industrial-grade nitrogen or the use of an open furnace, this fine atmosphere control can avoid the occurrence of oxidation reactions to the greatest extent, thereby reducing the internal stress and defects of the product.

[0042] In general, the invention scheme optimizes the system in multiple key links such as surface cleaning, heat treatment process, and protective atmosphere, and finally obtains high-quality aluminum nitride ceramic products with high surface cleanliness, good dimensional accuracy, and long service life. This innovative solution not only meets the semiconductor industry's stringent requirements for high-end materials, but also brings new development opportunities for downstream applications in this field.

[0043] Compared with some traditional simple sintering processes, this solution achieves an all-round improvement in product performance by giving full play to the synergistic effect of each link. For example, the fine cleaning in the early stage ensures the clean foundation for the subsequent high-temperature treatment; and the multiple fixture protection and precise temperature control in the later stage further improve the dimensional stability and stress level of the product. This collaborative optimization of the process not only improves the consistency of product quality, but also greatly reduces the defective rate in production.

[0044] In this embodiment, technicians are motivated to further optimize some details, such as exploring more efficient cleaning solvent formulations, or trying to use in-situ heat treatment and other technologies to further improve the energy efficiency of the process. At the same time, for some special application scenarios, the high temperature annealing process solution can also be adjusted in a targeted manner to further improve product performance and applicability.

[0045] For example, for some applications with more stringent requirements on surface finish, the surface cleaning process can be further optimized. In addition to the existing pure water-ethanol mixed solution and composite pickling solution, more advanced solvent formulas can be introduced, such as high-purity surfactants or supercritical fluids. This cleaning process upgrade is expected to further improve the finish of the ceramic surface while ensuring the decontamination effect, meeting more stringent cleanliness requirements.

[0046] For applications in some special process environments, the design of high-temperature annealing fixtures can also be optimized in a targeted manner. In addition to the existing solutions such as boron nitride liner and aluminum nitride shell, customized fixtures that better fit the sample geometry can also be considered. This optimization can further improve thermal conductivity, reduce local stress concentration, and ensure the dimensional accuracy and stability of ceramics under complex process conditions.

[0047] In addition, for some application scenarios that have more stringent requirements on the electrical properties of materials, the composition ratio of the high-temperature protective atmosphere can also be appropriately adjusted based on the existing process. In addition to using nitrogen with a purity of more than 99.999%, a small amount of hydrogen or other inert gases can also be appropriately added to further optimize the electrical insulation performance of the ceramic and meet more stringent electrical indicators.

[0048] In general, the invention has solved the key problems of aluminum nitride ceramics in high-temperature processing and has strong versatility and practicality. However, for some special application requirements, targeted optimization can still be carried out based on the existing process to further improve the applicability and competitiveness of the product in specific fields.

[0049] Example 4 The operating steps of the entire high temperature annealing process are as follows: First, the aluminum nitride ceramic sample to be processed is placed in a dedicated ultrasonic cleaning tank and a cleaning solution made of pure water and anhydrous ethanol is added. By precisely controlling the ultrasonic power and frequency, the ceramic surface is deeply cleaned to remove various particles and organic pollutants. This ultrasonic cleaning process usually lasts 10-15 minutes. After cleaning, the sample needs to be thoroughly rinsed with water-ethanol to ensure that the residual amount of detergent is minimized.

[0050] Then, the cleaned ceramic sample is transferred to the pickling tank and immersed in the pre-prepared HF-HNO3 composite acid solution. During the pickling process, appropriate stirring or ultrasonic oscillation should be applied to accelerate the dissolution of inorganic impurities on the surface. Pickling generally takes 20-30 minutes, after which it needs to be carefully rinsed with a large amount of pure water to ensure that there is no acid residue on the surface of the sample.

[0051] After cleaning and pickling, the sample can be placed in the reaction chamber of the high-temperature annealing furnace. A layer of boron nitride sintering fixture is placed at the bottom of the reaction chamber, and then the ceramic sample is placed on it. Two aluminum nitride ceramic fixtures are placed on the upper and lower sides of the sample, and an aluminum nitride block is pressed into the upper part. This "sandwich" multi-layer fixture design can effectively prevent the ceramic from deforming or warping at high temperatures.

[0052] After the sample and fixture are assembled in place, the high temperature annealing process can be started. First, the temperature of the reaction chamber is slowly raised to 1400-1500°C at a heating rate of 1-3°C / min. In this temperature range, the sample is kept warm for 2-4 hours to fully complete the microstructure adjustment and phase change process.

[0053] It is worth noting that the entire high-temperature annealing process is carried out in a nitrogen protective atmosphere with a purity of more than 99.999%. This ultra-high clean inert atmosphere can effectively block the entry of oxygen and other impurities in the air, ensuring that the ceramic will not undergo oxidation reaction at high temperatures.

[0054] After the insulation is completed, the reaction chamber begins to enter the cooling stage. The cooling rate in this stage is controlled at 3-5°C / min to slowly release thermal stress and avoid defects such as cracking of the ceramic during the rapid cooling process. The entire high-temperature annealing process, from heating to cooling, takes a total of 18-24 hours.

[0055] After the above-mentioned fine process, the surface roughness (Ra) of the aluminum nitride ceramic product finally obtained can be controlled within 0.1-0.3μm, and the internal residual stress level can be controlled below 50MPa. This excellent product performance not only meets the semiconductor industry's requirements for high cleanliness and high stability materials, but also lays the foundation for the wide application of this ceramic in this field.

[0056] In actual use, special attention should be paid to the following aspects: The first is strict control of the cleaning process. Surface cleanliness is the key foundation of the entire process. Any residual contaminants may lead to oxidation reactions or other defects during subsequent high-temperature treatment. Therefore, in ultrasonic cleaning and pickling treatment, various parameters must be strictly controlled, such as solvent ratio, pickling concentration, treatment time, etc., to ensure that the sample surface is thoroughly clean. At the same time, the water-ethanol rinse after each cleaning process should not be ignored to remove residual cleaning agents.

[0057] The second is the fixture protection design during high-temperature annealing. The multi-layer clamping fixture configuration can effectively prevent the ceramic from deforming or warping at high temperatures, but it also requires special attention in actual operation. First of all, the size matching between the layers of fixtures must be precise to avoid position deviation or excessive gaps that affect the heat conduction effect. At the same time, the roughness of the fixture surface must also be controlled within the range of Ra 0.6-Ra 0.4 to ensure good thermal conductivity and avoid local stress concentration. Only by doing these details can we truly achieve effective protection of ceramic samples.

[0058] The second is the precise control of temperature parameters. The process requires strict control of the temperature curve in each stage of heating, heat preservation and cooling. Any temperature exceeding the limit or too fast temperature rise / fall rate may lead to abnormal evolution of the microstructure, which in turn causes internal stress accumulation and defects. Therefore, in actual production, high-precision temperature sensors and PID control systems must be used to monitor and accurately adjust the furnace temperature in real time to ensure that the process parameters fully meet the requirements.

[0059] Finally, the protective atmosphere needs to be continuously maintained. This process uses nitrogen with a purity of more than 99.999% as the protective atmosphere, which can effectively block the influence of outside air. However, in actual operation, special attention should be paid to the stability and airtightness of the nitrogen flow. Once the nitrogen supply fluctuates or leaks, oxidation reactions may occur, resulting in a decrease in product quality. Therefore, strict gas monitoring and airtight protection measures must be taken to ensure the cleanliness and stability of the protective atmosphere throughout the high-temperature process.

[0060] Overall, the high-temperature annealing process demonstrates strong system integration and optimization capabilities. Through fine design of multiple key links such as cleaning process, high-temperature fixtures, temperature parameters, and protective atmosphere, the goal of high product cleanliness and stable performance was finally achieved. This innovative solution not only meets the semiconductor industry's stringent requirements for high-end materials, but also greatly enhances the application potential of aluminum nitride ceramics in this field.

[0061] From the perspective of feasibility, this process scheme fully integrates knowledge from multiple disciplines such as materials science, thermal engineering, process control, etc. The key technologies involved, such as ultrasonic cleaning, multi-layer fixture protection, and precise temperature control, have relatively mature theoretical foundations and process practices in related fields.

Claims

1. A high temperature annealing method for aluminum nitride ceramics, characterized in that: The following steps are involved: S1: Use anhydrous ethanol and pure water to clean the surface of aluminum nitride ceramics; S2: Immerse the product in a mixed acid solution prepared by HF and HNO3 for surface pickling; S3: placing the product in a solution of pure water and anhydrous ethanol for ultrasonic cleaning; S4: placing the cleaned aluminum nitride ceramic in a boron nitride fixture and placing it in a vacuum sintering furnace; S5: Annealing begins, the room temperature rises to 600°C, and the vacuum state is maintained; S6: Raise the temperature from 600°C to 1500°C, continue to introduce nitrogen, and keep warm after the temperature is raised; S7: Cool down to room temperature, continue to introduce nitrogen, and annealing is completed.

2. A high temperature annealing method for aluminum nitride ceramics according to claim 1, characterized in that: In the mixed acid solution described in S2, the HF concentration is 20%-30%, and the HNO3 concentration is 40%-50%.

3. A high temperature annealing method for aluminum nitride ceramics according to claim 1, characterized in that: The volume ratio of pure water to anhydrous ethanol described in S1 and S3 is 1:1 to 3:1, the ultrasonic intensity is 10-20W / In2, and the frequency is 35-45kHz.

4. A high temperature annealing method for aluminum nitride ceramics according to claim 1, characterized in that: The upper and lower sides of the boron nitride sintering jig in S4 are both provided with aluminum nitride ceramic jigs, and the aluminum nitride ceramic jig on the upper side of the boron nitride sintering jig is pressed with an aluminum nitride pressing block.

5. A high temperature annealing method for aluminum nitride ceramics according to claim 4, characterized in that: The surface roughness of the aluminum nitride ceramic fixture and the aluminum nitride compact is Ra0.6-Ra0.

4.

6. A high temperature annealing method for aluminum nitride ceramics according to claim 1, characterized in that: The heating rate from room temperature to 600°C in S5 is 1-3°C / min; the heating rate from 600°C to the highest temperature of 1300-1500°C is also 1-3°C / min.

7. A high temperature annealing method for aluminum nitride ceramics according to claim 1, characterized in that: The holding time at the highest temperature in S6 is 1-3 hours.

8. A high temperature annealing method for aluminum nitride ceramics according to claim 6, characterized in that: In S6 and S7, during the heating and insulation process, the flow rate of nitrogen introduced into the furnace is 10 NL / min.

9. A high temperature annealing method for aluminum nitride ceramics according to claim 1, characterized in that: The cooling rate in S7 is 0.5-2°C / min.

10. The high temperature annealing method for aluminum nitride ceramics according to any one of claims 1 to 9, characterized in that: The surface flatness of the aluminum nitride ceramic product after annealing is Ra≤0.4 μm, and the internal residual stress is reduced to ≤20 MPa.

Citation Information

Patent Citations

  • Preparation method of aluminum nitride ceramic with high heat conductivity

    CN107759225A

  • Method for recycling residual raw materials of PVT method-based aluminum nitride crystal growth

    CN113046834A

  • Aluminum nitride ceramic surface metallization method

    CN116986926A

  • Cleaning method of aluminum nitride ceramic

    CN117600143A

  • Aluminum nitride ceramic annealing sagger

    CN210180179U