Method for removing nanoparticles from silicon-based material

The protective layer is formed through low-energy plasma cleaning, atomic layer deposition and self-assembly technology, combined with dual-frequency ultrasonic assisted wet chemical cleaning, which solves the problems of low cleaning efficiency and surface damage in traditional methods, and achieves efficient nanoparticle removal and Surface protection.

CN119028810AInactive Publication Date: 2024-11-26BEIJING ZIGUANG HUATIAN THERMAL POWER TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411135546.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional method of removing nanoparticles of silicon-based materials has low cleaning efficiency, which can easily lead to some nanoparticles residues, and the cleaning method of high-energy plasma and chemical solution can easily damage the surface of silicon-based materials.

Method used

Low-energy plasma cleaning is used to form a nano-level protective layer combined with atomic layer deposition technology and self-assembly technology, and combined with dual-frequency ultrasonic-assisted wet chemical cleaning, gradually removing nanoparticles and reducing damage to the surface.

Benefits of technology

It significantly improves cleaning efficiency, reduces the risk of nanoparticle residue and surface damage, and ensures the integrity and chemical purity of the surface of silicon-based materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028810A_ABST
    Figure CN119028810A_ABST
Patent Text Reader

Abstract

The invention discloses a method for removing nano particles from a silicon-based material, and relates to the technical field of environmental protection, the method effectively reduces the dependence on a protective layer and reduces the risk of surface damage through low-energy plasma cleaning, electron temperature control and plasma density control and introduction of a local heating technology; a nanoscale protection layer is deposited on the surface by using an atomic layer deposition (ALD) technology before cleaning, and orderly arranged nanoparticles are formed through a self-assembly technology to provide additional protection; the double-frequency ultrasonic technology is introduced, cleaning is conducted by alternately using the frequency of 20 kHz and the frequency of 40 kHz, the cleaning effect is improved, and surface damage is reduced; in addition, deionized water is used for sufficient flushing after cleaning each time, nitrogen is used for drying, and surface chemical substance residues are reduced; the problems that in the prior art, wet chemical cleaning or single-frequency ultrasonic cleaning is depended on, and the cleaning efficiency is low are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection, and in particular to a method for removing nanoparticles from a silicon-based material. Background Art

[0002] Nanoscale contamination particles on the surface of silicon wafers can have a fatal impact on integrated circuit chip manufacturing. Cleaning and removing them is an important challenge facing the integrated circuit manufacturing industry. Especially when the node size gradually decreases, the impact of smaller-scale nanoparticles on chip performance will gradually increase, and the efficiency of traditional chemical cleaning methods will also be greatly reduced due to the reduction in node size. At the same time, more and more new materials are currently used in different links of the integrated circuit manufacturing process, which may lead to nanoparticle contamination with more new material components. Real-time monitoring of the composition of contaminated nanoparticles is conducive to quickly determining the source of pollution and timely warning and remediation of problems in various production links.

[0003] For example, the patent publication number CN108245995A discloses a method for efficiently removing nanoparticles from ordered mesoporous silicon-based materials, which belongs to the field of environmental protection technology. The method passes a large number of generated nanoparticles into a particle bed filter, and finally efficiently removes the nanoparticles. The particle bed filter contains spherical particles loaded with powdered ordered mesoporous silicon-based materials. The method has simple process conditions, cheap raw materials, and strong operability. It can provide a methodological basis and experimental foundation for source control of fine particulate matter in the atmosphere, and has good social value and theoretical significance.

[0004] Although the above scheme has the above advantages, the traditional method of removing nanoparticles from silicon-based materials relies on wet chemical cleaning or single-frequency ultrasonic cleaning, which has low cleaning efficiency and easily causes some nanoparticles to remain on the surface of the silicon-based material; and some cleaning methods using high-energy plasma and chemical solutions are prone to damage the surface of the silicon-based material during the cleaning process. Therefore, a method for removing nanoparticles from silicon-based materials is urgently needed to solve this problem. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for removing nanoparticles from silicon-based materials, which solves the problem that the prior art relies on wet chemical cleaning or single-frequency ultrasonic cleaning, which has low cleaning efficiency and easily causes some nanoparticles to remain on the surface of the silicon-based material; and some cleaning methods using high-energy plasma and chemical solutions easily damage the surface of the silicon-based material during the cleaning process.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] The present invention provides a method for removing nanoparticles from a silicon-based material, comprising:

[0008] Step 1. Pretreatment of the silicon-based surface to remove large-sized particles and organic pollutants on the surface of the silicon-based material; large-sized particles here are particles visible to the naked eye;

[0009] The silicon-based material is immersed in a cleaning solution, which is 99% isopropyl alcohol (IPA) and 99% ethanol, and then ultrasonic-assisted cleaning is performed for 5-10 minutes to remove surface organic pollutants; then the surface is fully rinsed with deionized water to remove residual organic solvents;

[0010] Step 2. Atomic layer deposition (ALD) of a nano-protective layer, depositing a nano-scale protective layer on the surface of the silicon-based material; using atomic layer deposition technology, depositing a layer of aluminum oxide (AI2O3) or silicon oxide (SiO2) on the surface of the silicon-based material; the deposition temperature is controlled at 150-200°C;

[0011] Step 3: Low-energy plasma cleaning: low-energy plasma is used for preliminary cleaning to remove surface nanoparticles;

[0012] Step 4. Ultrasonic-assisted wet chemical cleaning, combining ultrasonic waves and chemical solutions for deep cleaning to remove residual nanoparticles;

[0013] Use dual-frequency ultrasonic technology to improve cleaning efficiency and reduce damage to the surface; set two different frequencies of ultrasonic waves, 20kHz and 40kHz respectively; use the two frequencies of ultrasonic waves alternately for cleaning, and the cleaning time of each frequency is 3-5 minutes;

[0014] Step 5. Remove the protective layer. After cleaning, remove the protective layer on the surface to restore the surface state of the original silicon-based material.

[0015] The present invention is further configured as follows: before depositing the protective layer, a layer of orderly arranged nanoparticles is formed on the surface of the silicon-based material using a self-assembly technique:

[0016] Firstly, a nanoparticle suspension is prepared, wherein the nanoparticles are selected from silicon dioxide and aluminum oxide nanoparticles;

[0017] The nanoparticles are uniformly dispersed in an ethanol solution having a concentration of 0.1-1 mg / mL;

[0018] Ultrasonic treatment of the suspension for 5-10 min to evenly disperse the nanoparticles;

[0019] Dropping the prepared nanoparticle suspension on the surface of the silicon-based material;

[0020] The ambient temperature was controlled at 20-25°C, the humidity was maintained between 30-50%, and the solvent evaporation rate was maintained at 0.1-0.5 mL per minute;

[0021] Slowly dry at 50-60°C for 1-2 hours to allow the nanoparticles to adhere to the surface of the silicon-based material;

[0022] The present invention is further configured that the atomic layer deposition ALD method is:

[0023] Placing the self-assembled silicon-based material in a reaction chamber of an ALD device;

[0024] Alumina AI2O3 and silicon oxide SiO2 were selected as deposition materials, and the temperature of the reaction chamber was set at 150-200°C;

[0025] When aluminum oxide AI2O3 is used as the deposition material, trimethylaluminum TMA and water are used as precursors for deposition, with a TMA pulse of 0.1 second and an inert gas flushing of 20 seconds; a water pulse of 0.1 second and an inert gas flushing of 20 seconds;

[0026] Repeat the pulse cycle until the thickness reaches 2-5 nm;

[0027] When silicon oxide SiO2 is used as the deposition material, monosilane SiH4 and ozone O3 are used as precursors for deposition, with SiH4 pulse for 0.1 seconds and inert gas flushing for 20 seconds; O3 pulse for 0.1 seconds and inert gas flushing for 20 seconds;

[0028] Repeat the pulse cycle until the thickness reaches 2-5 nm;

[0029] The present invention is further configured that the plasma cleaning step comprises:

[0030] placing the silicon-based material deposited with the protective layer into a low-energy plasma cleaning device;

[0031] A low-energy, high-density RF plasma source is used to control the electron temperature at 2-5eV and the plasma density at 10 10 -10 11 cm -3 ;

[0032] Use a mixture of argon Ar and oxygen with a gas flow ratio of 9:1 for plasma cleaning for 10-20 minutes;

[0033] Improve plasma cleaning efficiency through local heating and reduce dependence on protective layers;

[0034] Add a local heating device to the plasma cleaning equipment and control the heating temperature at 100-150°C;

[0035] The present invention is further configured that the plasma cleaning method is:

[0036] Placing a silicon-based material for depositing a protective layer in a reaction chamber of a plasma cleaning device;

[0037] The RF power was set at 50-200W and the electron temperature was controlled at 2-5eV;

[0038] The plasma density was controlled by adjusting the RF power and gas flow rate. 10 -10 11 cm -3 ;

[0039] Using a mixture of argon and oxygen:

[0040] The Ar flow rate was set to 90 sccm, and the oxygen flow rate was set to 10 sccm;

[0041] Start the RF plasma source and turn on the supply of argon and oxygen mixed gas;

[0042] The cleaning time is controlled within 10-20 minutes;

[0043] Adding a local heating device to the plasma cleaning equipment to cover the sample surface;

[0044] The heating temperature is controlled at 100-150°C, and the heating time is synchronized with the plasma cleaning time;

[0045] The present invention is further configured that, after the low-energy plasma cleaning in step 3, the RF plasma source is turned off and the gas supply is stopped; the heating temperature is gradually reduced;

[0046] After the sample has cooled to room temperature, take out the silicon-based material;

[0047] The present invention is further configured that the ultrasonic-assisted wet chemical cleaning method in step 4 is:

[0048] Prepare chemical solutions and prepare solutions:

[0049] Take 1 mL of 48% hydrofluoric acid and dilute it to 100 mL of deionized water to get a 0.48% solution;

[0050] Take 5 mL of 68% nitric acid and dilute it to 100 mL of deionized water to get a 3.4% solution;

[0051] The hydrofluoric acid and nitric acid solutions of the above concentrations are mixed in a ratio of 1:1, and the concentration of hydrofluoric acid in the final solution is 0.5-1%, and the concentration of nitric acid is 1-5%;

[0052] The ultrasonic frequency range is set to 20-60kHz; the power is controlled at 100-200W;

[0053] Set up two ultrasonic waves with different frequencies, 20kHz and 40kHz;

[0054] Then wash it;

[0055] The present invention is further configured as follows:

[0056] The ultrasonic-assisted wet chemical cleaning method in step 4 also includes:

[0057] Pour the prepared chemical solution into the ultrasonic cleaning tank to cover the silicon-based material, and place the silicon-based material in the cleaning tank to immerse it in the solution;

[0058] Start the ultrasonic equipment and first use 20kHz frequency for cleaning;

[0059] The cleaning time is controlled within 3-5 minutes, then stop the 20kHz ultrasonic cleaning and switch to 40kHz frequency;

[0060] Clean again for 3-5 minutes with the ultrasonic power unchanged;

[0061] Alternately use two frequencies of ultrasonic waves for cleaning;

[0062] After cleaning, remove the silicon-based material from the solution, immediately rinse it in deionized water for 2-3 minutes, and blow dry the sample with nitrogen;

[0063] The present invention is further configured as follows:

[0064] The protective layer removal method in step 5 is:

[0065] Take 1 mL of 48% industrial grade hydrofluoric acid and add 99 mL of deionized water to obtain a 0.48% diluted solution;

[0066] Pour the diluted hydrofluoric acid solution into a corrosion-resistant container and fix it, fix the cleaned silicon-based material in the container, and immerse the surface completely in the hydrofluoric acid solution;

[0067] The soaking time is controlled within 1-3 minutes, and the temperature is maintained at 20-25℃ during the soaking process;

[0068] After soaking, remove the silicon-based material from the hydrofluoric acid solution and immediately rinse it in deionized water for 2-3 minutes;

[0069] After rinsing, the sample surface was blown dry with nitrogen.

[0070] Compared with the prior art, the present invention has the following beneficial effects:

[0071] The present invention uses low-energy plasma cleaning to control electron temperature and plasma density, and introduces local heating technology to effectively reduce dependence on the protective layer and reduce the risk of surface damage. A nano-scale protective layer is deposited on the surface using atomic layer deposition (ALD) technology before cleaning, and orderly arranged nanoparticles are formed through self-assembly technology to provide additional protection.

[0072] The present invention introduces dual-frequency ultrasonic technology, alternately uses 20kHz and 40kHz frequencies for cleaning, improves the cleaning effect, and reduces surface damage; and after each cleaning, it is fully rinsed with deionized water and blown dry with nitrogen to reduce the residual chemical substances on the surface;

[0073] The invention solves the problems existing in the prior art that the cleaning efficiency is low and some nanoparticles may remain on the surface of silicon-based materials, while some cleaning methods using high-energy plasma and chemical solutions may damage the surface of silicon-based materials during the cleaning process. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 The present invention is a flow chart of the method for removing nanoparticles from silicon-based materials. DETAILED DESCRIPTION

[0075] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0076] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0077] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0078] Example 1

[0079] See also Figure 1 The present invention provides a method for removing nanoparticles from a silicon-based material, comprising:

[0080] Step 1. Pretreatment of the silicon-based surface to remove large-sized particles and organic pollutants on the surface of the silicon-based material; large-sized particles here are particles visible to the naked eye;

[0081] The silicon-based material is immersed in a cleaning solution, which is 99% isopropyl alcohol (IPA) and 99% ethanol, and then ultrasonic-assisted cleaning is performed for 10 minutes to remove organic pollutants on the surface; then the surface is fully rinsed with deionized water to remove residual organic solvents;

[0082] Step 2. Atomic layer deposition (ALD) of a nano-protective layer, depositing a nano-scale protective layer on the surface of the silicon-based material; using atomic layer deposition technology, depositing a layer of aluminum oxide (AI2O3) or silicon oxide (SiO2) on the surface of the silicon-based material; the deposition temperature is controlled at 200°C;

[0083] Before depositing the protective layer, a layer of orderly arranged nanoparticles is formed on the surface of the silicon-based material using self-assembly technology:

[0084] Firstly, a nanoparticle suspension is prepared, wherein the nanoparticles are selected from silicon dioxide and aluminum oxide nanoparticles;

[0085] The nanoparticles are uniformly dispersed in an ethanol solution having a concentration of 0.1-1 mg / mL;

[0086] The suspension was treated with ultrasound for 10 min to evenly disperse the nanoparticles;

[0087] Dropping the prepared nanoparticle suspension on the surface of the silicon-based material;

[0088] The ambient temperature was controlled at 25°C, the humidity was maintained between 30%, and the solvent evaporation rate was maintained at 0.5 mL per minute;

[0089] Slow drying at 60°C for 2 hours allows the nanoparticles to adhere to the surface of the silicon-based material;

[0090] The Atomic Layer Deposition (ALD) method is:

[0091] Placing the self-assembled silicon-based material in a reaction chamber of an ALD device;

[0092] Silicon oxide SiO2 was used as the deposition material, and the temperature of the reaction chamber was set at 200°C;

[0093] Deposition was performed using monosilane SiH4 and ozone O3 as precursors, with SiH4 pulses of 0.1 seconds and inert gas flushing for 20 seconds; O3 pulses of 0.1 seconds and inert gas flushing for 20 seconds;

[0094] Repeat the pulse cycle until the thickness reaches 2-5 nm;

[0095] Step 3: Low-energy plasma cleaning: low-energy plasma is used for preliminary cleaning to remove surface nanoparticles;

[0096] Plasma cleaning steps include:

[0097] placing the silicon-based material deposited with the protective layer into a low-energy plasma cleaning device;

[0098] A low-energy, high-density RF plasma source is used to control the electron temperature at 5eV and the plasma density at 1011cm -3 ;

[0099] Plasma cleaning was performed for 20 minutes using a mixed gas of argon Ar and oxygen with a gas flow ratio of 9:1;

[0100] Improve plasma cleaning efficiency through local heating and reduce dependence on protective layers;

[0101] Add a local heating device to the plasma cleaning equipment and control the heating temperature at 150°C;

[0102] Plasma cleaning methods are:

[0103] Placing a silicon-based material for depositing a protective layer in a reaction chamber of a plasma cleaning device;

[0104] The RF power was set at 200 W, and the electron temperature was controlled at 5 eV;

[0105] The plasma density was controlled by adjusting the RF power and gas flow rate. 11 cm -3 ;

[0106] Using a mixture of argon and oxygen:

[0107] The Ar flow rate was set to 90 sccm, and the oxygen flow rate was set to 10 sccm;

[0108] Start the RF plasma source and turn on the supply of argon and oxygen mixed gas;

[0109] The cleaning time is controlled within 20 minutes;

[0110] Adding a local heating device to the plasma cleaning equipment to cover the sample surface;

[0111] The heating temperature is controlled at 150°C, and the heating time is synchronized with the plasma cleaning time;

[0112] Step 3: After low-energy plasma cleaning, turn off the RF plasma source and stop the gas supply; gradually reduce the heating temperature;

[0113] After the sample has cooled to room temperature, take out the silicon-based material;

[0114] Step 4. Ultrasonic-assisted wet chemical cleaning, combining ultrasonic waves and chemical solutions for deep cleaning to remove residual nanoparticles;

[0115] Use dual-frequency ultrasonic technology to improve cleaning efficiency and reduce damage to the surface; set two different frequencies of ultrasonic waves, 20kHz and 40kHz respectively; use the two frequencies of ultrasonic waves alternately for cleaning, and the cleaning time for each frequency is 5 minutes;

[0116] The ultrasonic-assisted wet chemical cleaning method in step 4 is:

[0117] Prepare chemical solutions and prepare solutions:

[0118] Take 1 mL of 48% hydrofluoric acid and dilute it to 100 mL of deionized water to get a 0.48% solution;

[0119] Take 5 mL of 68% nitric acid and dilute it to 100 mL of deionized water to get a 3.4% solution;

[0120] Mix the hydrofluoric acid and nitric acid solutions of the above concentrations in a ratio of 1:1;

[0121] Set up two ultrasonic waves with different frequencies, 20kHz and 40kHz;

[0122] Then wash it;

[0123] Pour the prepared chemical solution into the ultrasonic cleaning tank to cover the silicon-based material, and place the silicon-based material in the cleaning tank to immerse it in the solution;

[0124] Start the ultrasonic equipment and first use 20kHz frequency for cleaning;

[0125] The cleaning time is controlled within 3-5 minutes, then stop the 20kHz ultrasonic cleaning and switch to 40kHz frequency;

[0126] Clean again for 3-5 minutes with the ultrasonic power unchanged;

[0127] Alternately use two frequencies of ultrasonic waves for cleaning;

[0128] After cleaning, remove the silicon-based material from the solution, immediately rinse it in deionized water for 2-3 minutes, and blow dry the sample with nitrogen;

[0129] Step 5. Remove the protective layer. After cleaning, remove the protective layer on the surface to restore the surface state of the original silicon-based material.

[0130] The protective layer can be removed by:

[0131] Take 1 mL of 48% industrial grade hydrofluoric acid and add 99 mL of deionized water to obtain a 0.48% diluted solution;

[0132] Pour the diluted hydrofluoric acid solution into a corrosion-resistant container and fix it, fix the cleaned silicon-based material in the container, and immerse the surface completely in the hydrofluoric acid solution;

[0133] The soaking time is controlled within 3 minutes, and the temperature is maintained at 20-25℃ during the soaking process;

[0134] After soaking, remove the silicon-based material from the hydrofluoric acid solution and immediately rinse it in deionized water for 2-3 minutes;

[0135] After rinsing, the sample surface was blown dry with nitrogen.

[0136] Experimental example

[0137] Silicon-based material samples: Silicon-based material samples 1-5 with the same specifications and initial state were deployed and divided into an experimental group and a control group;

[0138] Cleaning equipment: ultrasonic cleaning equipment, plasma cleaning equipment, atomic layer deposition ALD equipment, local heating device;

[0139] Chemical reagents: 99% isopropyl alcohol IPA, 99% ethanol, hydrofluoric acid, nitric acid, deionized water;

[0140] Testing equipment: scanning electron microscope SEM, atomic force microscope AFM, X-ray photoelectron spectroscopy XPS, surface profiler;

[0141] Experimental procedures

[0142] Step 1: Surface preparation

[0143] 1. Experimental group: According to the cleaning method of Example 1, the silicon-based material sample was immersed in 99% IPA and 99% ethanol, and ultrasonic-assisted cleaning was performed for 10 minutes, and then the surface was fully rinsed with DI water;

[0144] 2. Control group: surface pretreatment was performed using wet chemical cleaning method;

[0145] Step 2: Atomic layer deposition (ALD) nano-protective layer

[0146] 1. Experimental group: According to the cleaning method of Example 1, a layer of orderly arranged nanoparticles is formed on the surface of the silicon-based material by self-assembly technology, and then atomic layer deposition is performed to deposit aluminum oxide or silicon oxide with a thickness controlled at 2-5 nanometers;

[0147] 2. Control group: No nanoparticle self-assembly was performed, and ALD deposition was performed directly;

[0148] Step 3: Low Energy Plasma Cleaning

[0149] 1. Experimental group: According to the cleaning method of Example 1, low-energy plasma cleaning was used and local heating was performed at the same time;

[0150] 2. Control group: using conventional plasma cleaning method without local heating;

[0151] Step 4: Ultrasonic assisted wet chemical cleaning

[0152] 1. Experimental group: cleaning was performed using dual-frequency ultrasonic technology and the chemical solution prepared in Example 1;

[0153] 2. Control group: single frequency ultrasonic cleaning;

[0154] Step 5: Remove the protective layer

[0155] 1. Experimental group: According to the cleaning method of Example 1, the protective layer was removed using a 0.5% diluted HF solution, followed by rinsing with DI water and drying with nitrogen gas;

[0156] 2. Control group: the protective layer was removed using the method of publication number CN108245995A;

[0157] Experimental results evaluation

[0158] Evaluation criteria:

[0159] 1. Cleaning efficiency: Observe the residual nanoparticles on the sample surface by scanning electron microscopy (SEM) and atomic force microscopy (AFM) to evaluate the cleanliness after cleaning;

[0160] 2. Surface integrity: Use AFM and surface profilometer to measure the roughness of the sample surface and evaluate the damage caused to the surface during the cleaning process;

[0161] 3. Chemical composition analysis: Analyze the chemical composition of the sample surface by X-ray photoelectron spectroscopy (XPS) to evaluate the chemical purity of the surface after cleaning;

[0162] Experimental data simulation

[0163] Table 1: Evaluation of cleaning efficiency (number of residual nanoparticles, unit: particles / μm 2 )

[0164]

[0165] Table 2: Surface integrity evaluation (surface roughness, unit: nm)

[0166]

[0167]

[0168] Table 3: Chemical composition analysis (residue content, unit: %)

[0169]

[0170] Experimental Summary

[0171] It can be seen from the above simulation experimental data that the solution provided in the present application is superior to the traditional method in terms of cleaning efficiency, surface integrity and chemical purity; the number of residual nanoparticles in the experimental group after cleaning is significantly reduced, the surface roughness is reduced, the content of chemical residues is reduced, and the cleaning effect consistency between batches is good; these data fully demonstrate the significant improvement of the solution of the present application in the removal of nanoparticles from silicon-based materials.

[0172] The method for removing nanoparticles from silicon-based materials provided in this application is intended to improve cleaning efficiency and protect the surface integrity of silicon-based materials;

[0173] First, the silicon-based material is immersed in 99% isopropyl alcohol (IPA) and 99% ethanol, and ultrasonic-assisted cleaning is performed for 5-10 minutes, and then the surface is fully rinsed with deionized water to remove residual organic solvents; then a nano-scale protective layer is deposited on the surface of the silicon-based material, and aluminum oxide or silicon oxide is deposited using atomic layer deposition technology; first, a nanoparticle suspension is prepared, silicon dioxide and aluminum oxide nanoparticles are selected, and uniformly dispersed in an ethanol solution, and the suspension is treated with ultrasound, and then the suspension is dropped on the surface of the silicon-based material, and warm drying is performed to make the nanoparticles adhere to the surface of the silicon-based material;

[0174] In the atomic layer deposition step, the self-assembled silicon-based material is placed in the reaction chamber of the ALD equipment, and aluminum oxide or silicon oxide is selected as the deposition material for pulsed cyclic deposition; low-energy plasma is used for preliminary cleaning to remove surface nanoparticles, and the silicon-based material with the deposited protective layer is placed in a low-energy plasma cleaning device, using a low-energy, high-density radio frequency RF plasma source and a mixed gas of argon and oxygen; local heating is used to improve the plasma cleaning efficiency;

[0175] In step 4, ultrasonic-assisted wet chemical cleaning is performed, combining ultrasonic waves and chemical solutions for deep cleaning to remove residual nanoparticles; dual-frequency ultrasonic technology is used to improve cleaning efficiency and reduce damage to the surface, and two different frequencies of ultrasonic waves are set, namely 20kHz and 40kHz, and the two frequencies are used alternately for cleaning, and the cleaning time for each frequency is 35 minutes;

[0176] After chemical cleaning, remove the protective layer, prepare a 0.48% diluted hydrofluoric acid solution, fix the cleaned silicon-based material in a corrosion-resistant container, and immerse the surface completely in the hydrofluoric acid solution. After the immersion, take out the silicon-based material, rinse it immediately in deionized water, and use nitrogen to blow dry the sample surface.

[0177] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for removing nanoparticles from silicon-based materials, characterized in that: include: Step 1. Pretreatment of the silicon-based surface to remove large-sized particles and organic pollutants on the surface of the silicon-based material; The silicon-based material is immersed in a cleaning solution, which is 99% isopropyl alcohol (IPA) and 99% ethanol, and then ultrasonic-assisted cleaning is performed for 5-10 minutes to remove surface organic pollutants; then the surface is fully rinsed with deionized water to remove residual organic solvents; Step 2. Atomic layer deposition (ALD) of a nano-protective layer, depositing a nano-scale protective layer on the surface of the silicon-based material; using atomic layer deposition technology, depositing a layer of aluminum oxide (AI2O3) or silicon oxide (SiO2) on the surface of the silicon-based material; the deposition temperature is controlled at 150-200°C; Step 3: Low-energy plasma cleaning: low-energy plasma is used for preliminary cleaning to remove surface nanoparticles; Step 4. Ultrasonic-assisted wet chemical cleaning, combining ultrasonic waves and chemical solutions for deep cleaning to remove residual nanoparticles; setting two different frequencies of ultrasonic waves, 20kHz and 40kHz respectively; alternating between the two frequencies of ultrasonic waves for cleaning, with each frequency cleaning time being 3-5 minutes; Step 5. Remove the protective layer. After cleaning, remove the protective layer on the surface to restore the surface state of the original silicon-based material.

2. The method for removing nanoparticles from silicon-based materials according to claim 1, characterized in that: Before depositing the protective layer, a layer of orderly arranged nanoparticles is formed on the surface of the silicon-based material using self-assembly technology: Firstly, a nanoparticle suspension is prepared, wherein the nanoparticles are selected from silicon dioxide and aluminum oxide nanoparticles; The nanoparticles are uniformly dispersed in an ethanol solution having a concentration of 0.1-1 mg / mL; Ultrasonic treatment of the suspension for 5-10 min to evenly disperse the nanoparticles; Dropping the prepared nanoparticle suspension on the surface of the silicon-based material; The ambient temperature was controlled at 20-25°C, the humidity was maintained between 30-50%, and the solvent evaporation rate was maintained at 0.1-0.5 mL per minute; Slowly dry at 50-60°C for 1-2 hours to allow the nanoparticles to adhere to the surface of the silicon-based material.

3. The method for removing nanoparticles from silicon-based materials according to claim 2, characterized in that: The Atomic Layer Deposition (ALD) method is: Placing the self-assembled silicon-based material in a reaction chamber of an ALD device; Alumina AI2O3 and silicon oxide SiO2 were selected as deposition materials, and the temperature of the reaction chamber was set at 150-200°C; When aluminum oxide AI2O3 is used as the deposition material, trimethylaluminum TMA and water are used as precursors for deposition, with a TMA pulse of 0.1 seconds and an inert gas flushing of 20 seconds; Water pulse 0.1 seconds, inert gas flushing 20 seconds; Repeat the pulse cycle until the thickness reaches 2-5 nm; When silicon oxide SiO2 is used as the deposition material, monosilane SiH4 and ozone O3 are used as precursors for deposition, with SiH4 pulse for 0.1 seconds and inert gas flushing for 20 seconds; O3 pulse for 0.1 seconds and inert gas flushing for 20 seconds; The pulse cycle was repeated until a thickness of 2-5 nm was achieved.

4. The method for removing nanoparticles from silicon-based materials according to claim 3, characterized in that: Plasma cleaning steps include: placing the silicon-based material deposited with the protective layer into a low-energy plasma cleaning device; A low-energy, high-density RF plasma source is used to control the electron temperature at 2-5eV and the plasma density at 10 10 -10 11 cm -3 ; Use a mixture of argon Ar and oxygen with a gas flow ratio of 9:1 for plasma cleaning for 10-20 minutes; Add a local heating device to the plasma cleaning equipment and control the heating temperature at 100-150℃.

5. The method for removing nanoparticles from silicon-based materials according to claim 4, characterized in that: Plasma cleaning methods are: Placing a silicon-based material for depositing a protective layer in a reaction chamber of a plasma cleaning device; The RF power was set at 50-200W and the electron temperature was controlled at 2-5eV; The plasma density was controlled by adjusting the RF power and gas flow rate. 10 -10 11 cm -3 ; Using a mixture of argon and oxygen: The Ar flow rate was set to 90 sccm, and the oxygen flow rate was set to 10 sccm; Start the RF plasma source and turn on the supply of argon and oxygen mixed gas; The cleaning time is controlled within 10-20 minutes; Adding a local heating device to the plasma cleaning equipment to cover the sample surface; The heating temperature is controlled at 100-150°C, and the heating time is synchronized with the plasma cleaning time.

6. The method for removing nanoparticles from silicon-based materials according to claim 5, characterized in that: Step 3: After low-energy plasma cleaning, turn off the RF plasma source and stop the gas supply; gradually reduce the heating temperature; wait for the sample to cool to room temperature and then take out the silicon-based material.

7. The method for removing nanoparticles from silicon-based materials according to claim 6, characterized in that: The ultrasonic-assisted wet chemical cleaning method in step 4 is: Prepare chemical solutions and prepare solutions: Take 1 mL of 48% hydrofluoric acid and dilute it to 100 mL of deionized water to get a 0.48% solution; Take 5 mL of 68% nitric acid and dilute it to 100 mL of deionized water to get a 3.4% solution; The hydrofluoric acid and nitric acid solutions of the above concentrations are mixed in a ratio of 1:1, and the concentration of hydrofluoric acid in the final solution is 0.5-1%, and the concentration of nitric acid is 1-5%; The ultrasonic frequency range is set to 20-60kHz; the power is controlled at 100-200W; Set up two ultrasonic waves with different frequencies, 20kHz and 40kHz; Then wash it.

8. The method for removing nanoparticles from silicon-based materials according to claim 7, characterized in that: The ultrasonic-assisted wet chemical cleaning method in step 4 also includes: Pour the prepared chemical solution into the ultrasonic cleaning tank to cover the silicon-based material, and place the silicon-based material in the cleaning tank to immerse it in the solution; Start the ultrasonic equipment and first use 20kHz frequency for cleaning; The cleaning time is controlled within 3-5 minutes, then stop the 20kHz ultrasonic cleaning and switch to 40kHz frequency; Clean again for 3-5 minutes with the ultrasonic power unchanged; Alternately use two frequencies of ultrasonic waves for cleaning; After cleaning, the silicon-based material was removed from the solution and immediately placed in deionized water for 2-3 minutes, and the sample was dried using nitrogen.

9. The method for removing nanoparticles from silicon-based materials according to claim 8, characterized in that: The protective layer removal method in step 5 is: Take 1 mL of 48% industrial grade hydrofluoric acid and add 99 mL of deionized water to obtain a 0.48% diluted solution; Pour the diluted hydrofluoric acid solution into a corrosion-resistant container and fix it, fix the cleaned silicon-based material in the container, and immerse the surface completely in the hydrofluoric acid solution; The soaking time is controlled within 1-3 minutes, and the temperature is maintained at 20-25℃ during the soaking process; After soaking, remove the silicon-based material from the hydrofluoric acid solution and immediately rinse it in deionized water for 2-3 minutes; After rinsing, the sample surface was blown dry with nitrogen.

Citation Information

Cited By

  • Cleaning method for electronic-grade polycrystalline silicon core

    CN119747292A

  • Method and equipment for treating residual soldering flux of soldering paste sintering process product

    CN120362184A

  • Ultrasonic cleaning process for gas diffuser

    CN121060879A