Composition, adhesive, cured product, and electronic component

By using a combination of epoxy resin, short-chain alkylsilyl fumed silica and high-viscosity thiol compounds in the adhesive, the problem of bleed-through of the adhesive during the heating and curing process is solved, and the quality of the finished product is improved. efficiency and reduce contamination of composition ingredients.

CN118725792APending Publication Date: 2024-10-01AJINOMOTO CO INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410333858.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing adhesive compositions containing epoxy resin are prone to bleeding during the heating and curing process, resulting in a reduction in yield, especially in the manufacturing of electronic equipment, which may lead to contamination of the components of the composition.

Method used

A composition containing an epoxy resin, a fumed silica having a short-chain alkylsilyl group, and a thiol compound exhibiting a viscosity of 0.2 Pa·s or more at 25° C. is used to inhibit the The occurrence of seepage.

Benefits of technology

It effectively suppresses the bleeding phenomenon during heat treatment, improves the yield, and reduces the contamination of composition components in the manufacturing of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004754417440000041
    Figure BDA0004754417440000041
  • Figure BDA0004754417440000051
    Figure BDA0004754417440000051
  • Figure BDA0004754417440000052
    Figure BDA0004754417440000052
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide an epoxy resin-containing composition that suppresses the occurrence of bleeding during heat treatment, an adhesive using the composition, a cured product of the composition, and an electronic component using the composition. The present disclosure provides a composition containing an epoxy resin, a fumed silica having at least one group selected from the group consisting of a dimethylsilyl group and a trimethylsilyl group, a curing accelerator, and a thiol compound exhibiting a viscosity of 0.2 Pa.s or more at 25 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a composition, an adhesive, a cured product, and an electronic component. Background Art

[0002] Epoxy resins are used in various applications such as adhesives. For example, Patent Document 1 below discloses a composition containing a specific epoxy resin, a specific thiol compound as a curing agent, a solid dispersion type latent curing accelerator, and a borate compound.

[0003] Prior art literature Patent Literature Patent Document 1: Japanese Patent Application Laid-Open No. 11-256013. Summary of the Invention

[0004] Technical problem to be solved by the invention When using as adhesive etc. the composition in the past that will comprise epoxy resin, in the coating portion of composition, contained composition in composition sometimes oozes out.The phenomenon that the composition of composition oozes out is usually referred to as bleed (bleed).The problem of this bleed manifests itself when heating when composition is cured especially.If bleed takes place when heat-curing, then the composition component can expand to originally unscheduled part, can cause the reduction of yield rate sometimes in the manufacturing of electronic equipment etc.For example, if bleed takes place near wiring, then the composition that oozes out from composition can pollute wiring.

[0005] The objects of the present disclosure include providing a composition containing an epoxy resin that suppresses the occurrence of bleeding during heat treatment, providing an adhesive using the composition, providing a cured product of the composition, and providing an electronic component using the composition.

[0006] Means of solving technical problems <1> A composition comprising: an epoxy resin, fumed silica having at least one group selected from dimethylsilyl and trimethylsilyl groups, a curing accelerator, and a thiol compound having a viscosity of 0.2 Pa·s or more at 25°C. <2> according to <1> The composition, wherein the viscosity of the thiol compound is in the range of 0.2 Pa·s to 15 Pa·s at 25°C. <3> according to <1> or <2> The composition, wherein the content of the fumed silica is within a range of 0.1% by mass to 20% by mass based on the total mass of the composition. <4> according to <1> ~ <3> The composition according to any one of the preceding claims, wherein the content of the thiol compound is within a range of 1% by mass to 80% by mass based on the total mass of the composition. <5> according to <1> ~ <4> The composition according to any one of the preceding claims, wherein the thiol compound does not have a ring skeleton. <6> according to <1> ~ <4> The composition according to any one of the preceding claims, wherein the thiol compound has a ring skeleton. <7> according to <1> ~ <6> The composition according to any one of the preceding claims, wherein the thiol compound does not have an ester bond. <8> An adhesive comprising <1> ~ <7> The composition of any one of the above. <9> A solidified material, which is <1> ~ <7> A cured product of any one of the compositions. <10> An electronic component comprising <9> The solidified material.

[0007] Effects of the Invention The present disclosure provides a composition containing an epoxy resin that suppresses the occurrence of bleed-out during heat treatment, an adhesive using the composition, a cured product of the composition, and an electronic component using the composition. DETAILED DESCRIPTION

[0008] Hereinafter, embodiments of the present disclosure will be described in detail. At least one of the following embodiments may be appropriately modified without departing from the spirit of the present disclosure.

[0009] <Composition> The composition of the present disclosure comprises the following components (A) to (D): (A) Epoxy resin (B) Fumed silica having at least one group selected from a dimethylsilyl group and a trimethylsilyl group (C) Curing accelerator (D) A thiol compound having a viscosity of 0.2 Pa·s or more at 25°C.

[0010] The composition comprising components (A) to (D) suppresses the occurrence of bleeding during heat treatment. It is speculated that this effect is mainly due to the use of a component (B) having a short-chain alkylsilyl group and a component (D) having a higher viscosity. It is believed that the component (D) showing a viscosity of 0.2 Pa·s or more at 25°C will suppress the occurrence of bleeding at lower temperatures (such as room temperature). Compared with long-chain alkylsilyl groups such as octylsilyl, the movement of short-chain alkylsilyl groups such as dimethylsilyl and trimethylsilyl is smaller even at higher temperatures. It is believed that the short-chain alkylsilyl group of component (B) has little effect on the viscosity of the composition during the heating process, so bleeding is difficult to occur even at higher temperatures. Therefore, it is believed that the composition comprising components (A) to (D) suppresses the occurrence of bleeding, especially the occurrence of bleeding during heat treatment.

[0011] (Epoxy resin) The composition contains an epoxy resin. One or more epoxy resins may be used.

[0012] The epoxy resin has at least one epoxy group. In a preferred embodiment, the epoxy resin comprises an epoxy resin having at least two epoxy groups.

[0013] The epoxy equivalent of the epoxy resin is preferably 40 g / eq to 10,000 g / eq, more preferably 50 g / eq to 8,000 g / eq, and even more preferably 60 g / eq to 5,000 g / eq. In this disclosure, "epoxy equivalent" refers to the mass of the epoxy resin per epoxy group, and the epoxy equivalent is measured in accordance with JIS K 7236 (2009).

[0014] The type of epoxy resin is not limited. The epoxy resin can be selected from epoxy resins used in known epoxy resin-containing compositions. Examples of epoxy resins include polyglycidyl ethers, glycidyl ether esters, polyglycidyl esters, epoxidized phenol novolac resins, epoxidized cresol novolac resins, epoxidized polyolefins, cycloaliphatic epoxy resins, and polyurethane-modified epoxy resins.

[0015] Examples of polyglycidyl ethers include reaction products of polyols and epichlorohydrin. Examples of polyols include polyphenols, glycerol, and polyethylene glycol. Examples of polyphenols include bisphenol A, bisphenol F, bisphenol AD, catechol, and resorcinol.

[0016] Examples of glycidyl ether esters include reaction products of hydroxycarboxylic acids and epichlorohydrin. Examples of hydroxycarboxylic acids include p-hydroxybenzoic acid and β-hydroxynaphthoic acid.

[0017] Examples of polyglycidyl esters include reaction products of polycarboxylic acids and epichlorohydrin. Examples of polycarboxylic acids include phthalic acid and terephthalic acid.

[0018] From the perspective of high heat resistance and low moisture permeability, in a preferred embodiment, the epoxy resin comprises at least one selected from bisphenol A epoxy resin, bisphenol F epoxy resin, phenol novolac epoxy resin, biphenyl aralkyl epoxy resin, phenol aralkyl epoxy resin, aromatic glycidylamine epoxy resin, and epoxy resin having a dicyclopentadiene structure. In a preferred embodiment, the epoxy resin comprises at least one selected from bisphenol A epoxy resin and bisphenol F epoxy resin.

[0019] The epoxy resin may be a liquid epoxy resin or a solid epoxy resin. Liquid epoxy resin is in a liquid state at 25°C. Solid epoxy resin is in a solid state at 25°C. Both liquid epoxy resin and solid epoxy resin may be used. In a preferred embodiment, the epoxy resin comprises a liquid epoxy resin. When the composition is used as an adhesive, it is preferably in a liquid state at 25°C. From the viewpoints of coating properties, processability, and adhesion, in a preferred embodiment, at least 50% by mass, preferably 60% by mass, more preferably 70% by mass, more preferably 80% by mass, more preferably 90% by mass, and particularly preferably 100% by mass of the total mass of the epoxy resin is liquid epoxy resin.

[0020] Examples of liquid epoxy resins include bisphenol A epoxy resins (e.g., "jER828EL," "jER827," and "YL980" manufactured by Mitsubishi Chemical Corporation), bisphenol F epoxy resins (e.g., "jER807" manufactured by Mitsubishi Chemical Corporation), naphthalene-type difunctional epoxy resins (e.g., "HP4032" and "HP4032D" manufactured by DIC Corporation), mixtures of bisphenol A epoxy resins and bisphenol F epoxy resins (e.g., "ZX-1059" manufactured by Nippon Steel Chemicals Co., Ltd.), and epoxy resins with hydrogenated structures (e.g., "jERYX8000" manufactured by Mitsubishi Chemical Corporation). Commercially available examples of liquid epoxy resins include "YX7105" (manufactured by Mitsubishi Chemical Corporation) and "EXA-4850-150" (manufactured by DIC Corporation).

[0021] Examples of solid epoxy resins include naphthalene-type tetrafunctional epoxy resins (e.g., “HP4700” manufactured by DIC Corporation), dicyclopentadiene-type multifunctional epoxy resins (e.g., “HP7200” manufactured by DIC Corporation), naphthol-type epoxy resins (e.g., “ESN-475V” manufactured by Nippon Steel Chemicals Co., Ltd.), epoxy resins having a butadiene structure (e.g., “PB-3600” manufactured by Daicel Corporation), and epoxy resins having a biphenyl structure (e.g., “NC3000H” and “NC3000L” manufactured by Nippon Kayaku Co., Ltd. or “jERYX4000” manufactured by Mitsubishi Chemical Corporation).

[0022] The epoxy resin may contain a linear hydrocarbon structural unit having 4 or more carbon atoms and / or a polyalkylene ether structural unit having 3 or more ether oxygen atoms. An example of a linear hydrocarbon structural unit having 4 or more carbon atoms is -(CH2) x -. x is 4 or greater. x may be in the range of 4 to 20 or 4 to 10. The number of ether oxygen atoms in the polyalkylene ether structural unit may be in the range of 3 to 20 or 3 to 10.

[0023] The epoxy resin may be an epoxy resin represented by the following formula (1) or the following formula (2).

[0024] [Chemical Formula 1]

[0025] In formula (1) and formula (2), X, X1, and X2 are each independently a divalent non-aromatic hydrocarbon group containing at least four -(CH2)- groups constituting the main backbone of the epoxy resin, Ar, Ar1, and Ar2 are each independently a divalent hydrocarbon group containing a divalent aromatic group constituting the main backbone of the epoxy resin, and n and m are each independently an integer from 1 to 20. The "main backbone of the epoxy resin" refers to the longest backbone connecting the two epoxy groups located at the ends of the epoxy resin.

[0026] In a preferred embodiment, the "divalent non-aromatic hydrocarbon group containing at least 4 -(CH2)-" in X, X1 and X2 is selected from -O-CH(-CH3)-(O-(CH2) p ) q -O-CH(-CH3)-、-(O-(CH2) r ) s -、-(O-CH2-CH3) t -, -O-CH2-CH(-OH)-CH2-(O-(CH2) u ) v -O-CH2-CH(-OH)-CH2-、-(O-(CH2) w ) y -O-CH2-CH(-OH)- and -(O-CH2-CH(-CH3)) z -O-CH2-CH(-OH)-, p, q, r, s, t, u, v, w, y and z are each independently an integer of 1 to 20.

[0027] Regarding the “divalent hydrocarbon group containing a divalent aromatic group” in Ar, Ar1 and Ar2, examples of aromatic groups include phenylene, naphthyl, anthracenyl and biphenylene. Phenylene may be o-phenylene, m-phenylene or p-phenylene. The hydrocarbon group may contain two or more aromatic groups. In the case where the hydrocarbon group contains two or more aromatic groups, the aromatic groups may be directly bonded to each other. The aromatic groups may also be bonded to each other via an alkylene group, an ether bond, an ester bond, an amide bond or two carbon atoms bonded by a double bond or a triple bond. Examples of preferred divalent hydrocarbon groups include divalent hydrocarbon groups represented by the following formula (3) or the following formula (4).

[0028] [Chemical Formula 2]

[0029] The epoxy resin may be a modified bisphenol-type epoxy resin represented by the following formula (5).

[0030] [Chemical Formula 3]

[0031] In formula (5), Y is an aliphatic hydrocarbon, Z is CH2 or C(CH3), and n is 0 to 10, preferably 1 to 8.

[0032] The epoxy resin may be a flexible epoxy resin. Examples of commercially available flexible epoxy resins include "YX7105" (Mitsubishi Chemical Corporation), "YX7110" (Mitsubishi Chemical Corporation), "YX7400" (Mitsubishi Chemical Corporation), and "EXA-4850-150" (DIC Corporation).

[0033] Based on the total mass of the composition, the content of the epoxy resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more. Furthermore, based on the total mass of the composition, the content of the epoxy resin is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more. Based on the total mass of the composition, the content of the epoxy resin is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. Furthermore, based on the total mass of the composition, the content of the epoxy resin is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. For example, based on the total mass of the composition, the content of the epoxy resin may be in the range of 5% to 95% by mass.

[0034] (Fumed Silica) The composition contains fumed silica having at least one group selected from a dimethylsilyl group and a trimethylsilyl group. One or more fumed silicas can be used.

[0035] In a preferred embodiment, at least one group selected from dimethylsilyl and trimethylsilyl groups is present at least on the surface of the fumed silica. The dimethylsilyl and trimethylsilyl groups in the fumed silica can be detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0036] Examples of methods for introducing dimethylsilyl or trimethylsilyl groups into fumed silica include surface treatment using a compound having a dimethylsilyl or trimethylsilyl group. Examples of compounds having a dimethylsilyl group include dimethyldichlorosilane. Examples of compounds having a trimethylsilyl group include hexamethyldisilazane.

[0037] In a preferred embodiment, the specific surface area of ​​the fumed silica is 5 m 2 / g~500m 2 The lower limit of the above specific surface area can be 40m 2 / g, 20m 2 / g or 10m 2 / g. The upper limit of the above specific surface area may be 200m 2 / g、300m 2 / g or 400m 2 In the present disclosure, the specific surface area is measured by BET (nitrogen adsorption method).

[0038] Examples of commercially available products of fumed silica include "RX300" (manufactured by Nippon Aerosil Corporation), "R976S" (manufactured by Nippon Aerosil Corporation), and "R974" (manufactured by Nippon Aerosil Corporation).

[0039] From the viewpoint of further suppressing the occurrence of seepage material, in a preferred embodiment, based on the gross mass of the composition, the content of fumed silica is in the range of 0.1 mass % to 20 mass %. The lower limit of the above content is preferably 2 mass %, more preferably 3 mass %, and further preferably 5 mass %. The upper limit of the above content is preferably 18 mass %, more preferably 16 mass %, and further preferably 14 mass %.

[0040] (Curing Accelerator) The composition contains a curing accelerator. One or more curing accelerators may be used.

[0041] The type of curing accelerator is not limited. The curing accelerator can be selected from the curing accelerators used in the known compositions containing epoxy resins. In a preferred embodiment, the curing accelerator comprises a latent curing accelerator. The latent curing accelerator is a compound that does not contribute to the curing of the epoxy resin at room temperature (25° C.) but promotes the curing of the epoxy resin when heated.

[0042] In a preferred embodiment, the latent curing accelerator is a solid-dispersible latent curing accelerator. A solid-dispersible latent curing accelerator is a compound that is insoluble in epoxy resin at room temperature (25°C) and becomes solubilized upon heating to act as a curing accelerator for the epoxy resin. Examples of solid-dispersible latent curing accelerators include imidazole compounds that are solid at 25°C and solid-dispersible amine adduct-based latent curing accelerators. Preferred are solid-dispersible amine adduct-based latent curing accelerators.

[0043] Examples of imidazole compounds that are solid at 25° C. include 2-heptadecylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-undecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2-methylimidazolyl-(1))-ethyl-s-triazine, 2,4-diamino-6-(2′-methylimidazolyl-(1))-ethyl-s-triazine, ')-ethyl-s-triazine / isocyanuric acid adduct, 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole-trimellitate, 1-cyanoethyl-2-phenylimidazole-trimellitate, N-(2-methylimidazolyl-1-ethyl)-urea, and N,N'-(2-methylimidazolyl-(1)-ethyl)-adipic acid diamide.

[0044] Examples of the solid dispersion-type amine adduct-based latent curing accelerator include reaction products of an amine compound and an epoxy compound, and reaction products of an amine compound and an isocyanate compound or a urea compound.

[0045] Examples of amine compounds used as raw materials for solid-dispersible amine adduct-based latent curing accelerators include compounds having at least one active hydrogen atom capable of addition-reacting with an epoxy group and at least one amino group selected from primary, secondary, and tertiary amino groups. Examples of such amine compounds include aliphatic amines (e.g., diethylenetriamine, triethylenetetramine, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diaminodicyclohexylmethane), aromatic amine compounds (e.g., 4,4'-diaminodiphenylmethane and 2-methylaniline), and nitrogen-containing heterocyclic compounds (e.g., 2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazoline, 2,4-dimethylimidazoline, piperidine, and piperazine).

[0046] Amine compounds having a tertiary amino group in the molecule are raw materials for providing latent curing accelerators having excellent curing accelerating ability. Examples of such compounds include dimethylaminopropylamine, diethylaminopropylamine, di-n-propylaminopropylamine, dibutylaminopropylamine, dimethylaminoethylamine, diethylaminoethylamine, N-methylpiperazine, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-dimethylaminoethanol, 1-methyl-2-dimethylaminoethanol, 1-phenoxymethyl-2-dimethylaminoethanol, 2-diethylaminoethanol, 1-butoxymethyl-2-dimethylaminoethanol, 1-(2-hydroxy-3-phenoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2-methyl imidazole, 1-(2-hydroxy-3-butoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-phenylimidazoline, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazoline, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N-β-hydroxyethylmorpholine, 2-dimethylaminoethanethiol, 2-mercaptopyridine, 2-benzimidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 4-mercaptopyridine, N,N-dimethylaminobenzoic acid, N,N-dimethylglycine, nicotinic acid, isonicotinic acid, picolinic acid, N,N-dimethylglycine hydrazide, N,N-dimethylpropionyl hydrazide, nicotinyl hydrazide, and isonicotinyl hydrazide.

[0047] Examples of epoxy compounds used as raw materials for solid-dispersible amine adduct-based latent curing accelerators include polyglycidyl ethers, glycidyl ether esters, polyglycidyl esters, glycidyl amine compounds, epoxidized phenol novolac resins, epoxidized cresol novolac resins, epoxidized polyolefins, butyl glycidyl ether, phenyl glycidyl ether, and glycidyl methacrylate. The epoxy compound may have one epoxy group or at least two epoxy groups.

[0048] Examples of polyglycidyl ethers include reaction products of polyols and epichlorohydrin. Examples of polyols include polyphenols, glycerol, and polyethylene glycol. Examples of polyphenols include bisphenol A, bisphenol F, catechol, and resorcinol.

[0049] Examples of glycidyl ether esters include reaction products of hydroxycarboxylic acids and epichlorohydrin. Examples of hydroxycarboxylic acids include p-hydroxybenzoic acid and β-hydroxynaphthoic acid.

[0050] Examples of polyglycidyl esters include reaction products of polycarboxylic acids and epichlorohydrin. Examples of polycarboxylic acids include phthalic acid and terephthalic acid.

[0051] Examples of the glycidylamine compound include reaction products of 4,4'-diaminodiphenylmethane or m-aminophenol and epichlorohydrin.

[0052] When a latent curing accelerator is produced by reacting an amine compound with an epoxy compound, an active hydrogen compound having at least two active hydrogen atoms in the molecule may be added. Examples of active hydrogen compounds include polyphenols (e.g., bisphenol A, bisphenol F, bisphenol S, hydroquinone, catechol, resorcinol, pyrogallol, and novolac resins), polyols (e.g., trimethylolpropane), polycarboxylic acids (e.g., adipic acid and phthalic acid), 1,2-dimercaptoethane, 2-mercaptoethanol, 1-mercapto-3-phenoxy-2-propanol, thioglycolic acid, anthranilic acid, and lactic acid.

[0053] Examples of isocyanate compounds used as raw materials for solid-dispersible amine adduct-based latent curing accelerators include monofunctional isocyanate compounds (e.g., n-butyl isocyanate, isopropyl isocyanate, phenyl isocyanate, and benzyl isocyanate), polyfunctional isocyanate compounds (e.g., hexamethylene diisocyanate, toluene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, xylylene diisocyanate, p-phenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, and bicycloheptane triisocyanate), and compounds containing terminal isocyanate groups obtained by reacting polyfunctional isocyanate compounds with active hydrogen compounds. Examples of compounds containing terminal isocyanate groups include addition compounds containing terminal isocyanate groups obtained by reacting toluene diisocyanate with trimethylolpropane, and addition compounds containing terminal isocyanate groups obtained by reacting toluene diisocyanate with pentaerythritol.

[0054] Examples of the urea compound used as a raw material for the solid dispersion type amine adduct-based latent curing accelerator include urea and thiourea.

[0055] Examples of commercially available products of the reaction product of an amine compound and an epoxy compound include “Ajicure PN-40J” (manufactured by Ajinomoto Fine-Techno Co., Inc.), “Ajicure PN-F” (manufactured by Ajinomoto Fine-Techno Co., Inc.), “Ajicure PN-23” (manufactured by Ajinomoto Fine-Techno Co., Ltd.), “Ajicure PN-H” (manufactured by Ajinomoto Fine-Techno Co., Ltd.), “Novacure HX-3742” (manufactured by Asahi Kasei Corporation), and “Novacure HX-3721” (manufactured by Asahi Kasei Corporation).

[0056] Examples of commercially available products of the reaction product of an amine compound and an isocyanate compound or a urea compound include "FujiCure FXR-1020" (manufactured by Fuji Chemical Co., Ltd.) and "FujiCure FXR-1030" (manufactured by Fuji Chemical Co., Ltd.).

[0057] The content of the curing accelerator is preferably within a range of 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, and even more preferably 0.5 to 5% by mass, based on the total mass of the composition.

[0058] The ratio of the total mass of the curing accelerator to the total mass of the epoxy resin is preferably 0.1 to 100 mass%, more preferably 1 to 60 mass%, and even more preferably 5 to 30 mass%.

[0059] (Thiol compound) The composition contains a thiol compound having a viscosity of 0.2 Pa·s or more at 25° C. One or more thiol compounds may be used.

[0060] The viscosity of the thiol compound is 0.2 Pa·s or more at 25°C. From the viewpoint of further suppressing the occurrence of bleeding, the lower limit of the viscosity of the thiol compound is preferably 0.4 Pa·s, more preferably 0.6 Pa·s, and further preferably 0.8 Pa·s. The lower limit of the viscosity of the thiol compound may be 1 Pa·s or 3 Pa·s. The upper limit of the viscosity of the thiol compound is preferably 40 Pa·s, more preferably 20 Pa·s, and further preferably 15 Pa·s. The upper limit of the viscosity of the thiol compound may be 10 Pa·s, 8 Pa·s, or 6 Pa·s. For example, the viscosity of the thiol compound may be in the range of 0.2 Pa·s to 40 Pa·s at 25°C. In the present disclosure, the viscosity of the thiol compound is measured by a rheometer.

[0061] Examples of the thiol compound include tris(3-mercaptopropyl)isocyanurate (abbreviation: TMPIC), pentaerythritol tetrakis(3-mercaptobutyrate) (e.g., "Karenz MT (registered trademark) PE1" manufactured by RESONAC), and pentaerythritol tripropanethiol (e.g., "Multhiol Y-3" manufactured by SC Organic Chemicals).

[0062] The molecular weight of the thiol compound is preferably in the range of 200 to 700, more preferably 250 to 500, and even more preferably 300 to 400.

[0063] The thiol compound has at least one thiol group. In a preferred embodiment, the thiol compound includes a compound having at least two thiol groups. The number of thiol groups in the thiol compound is preferably 2 to 6, more preferably 3 to 6, and even more preferably 3 to 5. Furthermore, the number of thiol groups in the thiol compound is preferably 3 or 4, and more preferably 3.

[0064] The thiol equivalent weight of the thiol compound is preferably in the range of 50 g / eq to 400 g / eq, more preferably in the range of 50 g / eq to 300 g / eq, and even more preferably in the range of 70 g / eq to 200 g / eq. Furthermore, the thiol equivalent weight of the thiol compound is preferably in the range of 80 g / eq to 150 g / eq. In this disclosure, "thiol equivalent weight" refers to the mass of the thiol compound per thiol group.

[0065] In a preferred embodiment, the thiol compound does not have an ester bond. An ester bond is a bond represented by "-C(=O)O-." Since hydrolysis due to the ester bond does not occur, moisture resistance is improved and reliability is increased.

[0066] In a preferred embodiment, the thiol compound does not have a hydroxyl group. A thiol compound without a hydroxyl group can improve the pot life of the composition. As a result, the composition can achieve both pot life and rapid curing properties.

[0067] In a preferred embodiment, the thiol compound does not have a ring skeleton. When the thiol compound does not have a ring skeleton, the skeleton of the thiol compound becomes soft, and the peel strength can be improved.

[0068] In a preferred embodiment, the thiol compound has a cyclic skeleton. A thiol compound having a cyclic skeleton can improve shear adhesion. The thiol compound having a cyclic skeleton can be a monocyclic compound or a polycyclic compound. Examples of the cyclic skeleton include alicyclic skeletons, aromatic skeletons, and heterocyclic skeletons. The cyclic skeleton is preferably an aromatic skeleton or a heterocyclic skeleton, more preferably a heterocyclic skeleton. Examples of heterocyclic skeletons include: heterocyclic skeletons having 5- to 8-membered rings containing at least one nitrogen atom. Specifically, examples of heterocyclic skeletons include isocyanuric acid skeletons and glycoluril skeletons.

[0069] In a preferred embodiment, the thiol compound includes a compound represented by the following formula (6).

[0070] [Chemical Formula 4]

[0071] In formula (6), R1, R2, and R3 each independently represent a linear or branched divalent hydrocarbon group having 1 to 6 carbon atoms, preferably 1 to 5 carbon atoms. The hydrocarbon group may include divalent groups shown in (6a) to (6c) below. The number of divalent groups may be 1 or 2 or more.

[0072] [Chemical Formula 5]

[0073] Examples of the compound represented by formula (6) include tris(3-mercaptopropyl)isocyanurate (abbreviation: TMPIC).

[0074] From the viewpoint of the curability of the composition, in a preferred embodiment, the ratio of the number of thiol groups of the thiol compound to the number of epoxy groups of the epoxy resin (total thiol groups of the thiol compound / total epoxy groups of the epoxy resin) is preferably 0.1 to 2.0, more preferably 0.5 to 1.2. The "number of epoxy groups" represents the value obtained by dividing the mass of the epoxy resin contained in the composition by the epoxy equivalent (the mass of the epoxy group / the epoxy equivalent). It should be noted that when a plurality of epoxy resins are included in the composition, the number of epoxy groups represents the sum of the values ​​obtained by dividing the mass of each epoxy resin by the equivalent of each epoxy group. The "number of thiol groups" represents the value obtained by dividing the mass of the thiol contained in the composition by the thiol equivalent (the mass of the thiol group / the thiol equivalent). It should be noted that when a plurality of thiols are included in the composition, the number of thiol groups represents the sum of the values ​​obtained by dividing the mass of each thiol by the equivalent of each thiol. In the case where the composition contains a thiol compound other than "a thiol compound showing a viscosity of 0.2 Pa·s or more at 25° C.", the above ratio can be calculated based on the number of thiol groups of all thiol compounds contained in the composition.

[0075] From the viewpoint of further suppressing the occurrence of seepage material, in a preferred embodiment, based on the gross mass of the composition, the content of the thiol compound is in the range of 1 mass % to 80 mass %. The lower limit of the above-mentioned content is preferably 3 mass %, more preferably 5 mass %, and further preferably 7 mass %. The upper limit of the above-mentioned content is preferably 75 mass %, more preferably 70 mass %, and further preferably 60 mass %.

[0076] (Stabilizer) The composition may further contain a stabilizer. The stabilizer can improve the storage stability of the composition. One or more storage stabilizers may be used.

[0077] Examples of stabilizers include borate compounds, titanate compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids. In a preferred embodiment, the composition includes at least one stabilizer selected from borate compounds, titanate compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids.

[0078] Examples of the borate ester compound include trimethyl borate, triethyl borate, tri-n-propyl borate, tri-isopropyl borate, tri-n-butyl borate, tripentyl borate, triallyl borate, trihexyl borate, tricyclohexyl borate, trioctyl borate, trinonyl borate, tridecyl borate, tridodecyl borate, trihexadecyl borate, trioctadecyl borate, tris(2-ethylhexyloxy)borane, bis(1,4,7,10-tetraoxaundecyl)(1,4,7,10,13-pentaoxatetradecyl)(1,4,7-trioxaundecyl)borane, tribenzyl borate, triphenyl borate, tri-o-cresyl borate, tri-m-cresyl borate, and triethanolamine borate.

[0079] Examples of the titanate compound include tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, and tetraoctyl titanate.

[0080] Examples of the aluminate compound include triethyl aluminate, tripropyl aluminate, triisopropyl aluminate, tributyl aluminate, and trioctyl aluminate.

[0081] Examples of the zirconate compound include tetraethyl zirconate, tetrapropyl zirconate, tetraisopropyl zirconate, and tetrabutyl zirconate.

[0082] Examples of the isocyanate compound include n-butyl isocyanate, isopropyl isocyanate, 2-chloroethyl isocyanate, phenyl isocyanate, p-chlorophenyl isocyanate, benzyl isocyanate, hexamethylene diisocyanate, 2-ethylphenyl isocyanate, 2,6-dimethylphenyl isocyanate, 2,4-toluene diisocyanate, toluene diisocyanate, 2,6-toluene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4′-diisocyanate, tolidine diisocyanate, isophorone diisocyanate, xylylene diisocyanate, p-phenylene diisocyanate, and dicycloheptane triisocyanate.

[0083] Examples of carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, hexanoic acid, octanoic acid, acrylic acid, methacrylic acid, crotonic acid, monochloroacetic acid, dichloroacetic acid, glycolic acid, lactic acid, glyoxylic acid, tartaric acid, oxalic acid, malonic acid, succinic acid, maleic acid, benzoic acid, halogenated benzoic acid, methylbenzoic acid, phenylacetic acid, cinnamic acid, mandelic acid, phthalic acid, and trimesic acid.

[0084] Examples of the acid anhydride include succinic anhydride, dodecenylsuccinic anhydride, maleic anhydride, an adduct of methylcyclopentadiene and maleic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride.

[0085] Examples of the mercapto organic acid include mercaptoacetic acid, mercaptopropionic acid, mercaptobutyric acid, mercaptosuccinic acid, dimercaptosuccinic acid, mercaptoaliphatic monocarboxylic acids obtained by esterification of a hydroxy organic acid with a mercapto organic acid, and mercaptoaromatic monocarboxylic acids (eg, mercaptobenzoic acid).

[0086] From the viewpoints of versatility, safety, and storage stability of the composition, the stabilizer is preferably a borate ester compound, more preferably triethyl borate, tri-n-propyl borate, triisopropyl borate, or tri-n-butyl borate, and still more preferably triethyl borate.

[0087] The content of the stabilizer is preferably within a range of 0.0005% by mass to 30% by mass, more preferably 0.02% by mass to 20% by mass, and even more preferably 0.1% by mass to 10% by mass, based on the total mass of the composition.

[0088] (Other ingredients) The composition may further contain other components as needed. Examples of other components include diluents, solvents, pigments, flexibility-imparting agents, coupling agents, antioxidants, thixotropy-imparting agents, and dispersants.

[0089] Without departing from the scope of the purport of the present disclosure, composition can include the fumed silica without dimethylsilyl and trimethylsilyl.But, from the viewpoint of further suppressing the generation of infiltration material, preferably, reduce the containing rate of the fumed silica without dimethylsilyl and trimethylsilyl.Relative to the gross mass of the fumed silica contained in the composition, the containing rate of the fumed silica without dimethylsilyl and trimethylsilyl is preferably 50 mass % or less, more preferably 40 mass % or less, more preferably 30 mass % or less, more preferably 20 mass % or less, more preferably 10 mass % or less, more preferably 5 mass % or less, particularly preferably 0 mass %.In a preferred embodiment, composition does not include the fumed silica without dimethylsilyl and trimethylsilyl.Without departing from the scope of the purport of the present disclosure, composition can include the inorganic filler other than the fumed silica of silicon dioxide, calcium carbonate, aluminum oxide, zirconium oxide, aluminum nitride etc.

[0090] Without departing from the scope of the present disclosure, the composition may include a thiol compound that shows a viscosity of less than 0.2 Pa s at 25°C. However, from the viewpoint of further suppressing the occurrence of bleeding, it is preferred to reduce the content of the thiol compound that shows a viscosity of less than 0.2 Pa s at 25°C. Based on the total mass of the composition, the content of the thiol compound that shows a viscosity of less than 0.2 Pa s at 25°C is preferably 0% by mass to 3% by mass, more preferably 0% by mass to 1% by mass, and further preferably in the range of 0% by mass to 0.1% by mass. From the viewpoint of further suppressing the occurrence of bleeding, the ratio of the total mass of the thiol compounds that show a viscosity of less than 0.2 Pa s at 25°C to the total mass of the thiol compounds that show a viscosity of 0.2 Pa s or more at 25°C is preferably 0% by mass to 5% by mass, more preferably 0% by mass to 3% by mass, and further preferably in the range of 0% by mass to 1% by mass. In a preferred embodiment, the composition does not include a thiol compound that shows a viscosity of less than 0.2 Pa s at 25°C.

[0091] Composition can comprise organic solvent.But, from the viewpoint of the generation that suppresses seepage material, preferably, reduce the containing ratio of organic solvent.With the gross mass of composition as benchmark, the containing ratio of organic solvent is preferably below 5 mass %, more preferably below 3 mass %, further preferably below 1 mass %, further preferably below 0.1 mass %, particularly preferably 0 mass %.In a preferred embodiment, composition does not comprise organic solvent.

[0092] (Characteristics of the composition) In a preferred embodiment, the composition is a liquid composition having fluidity at 25°C.

[0093] In a preferred embodiment, the composition exhibits a viscosity within the range of 1 Pa·s to 200 Pa·s under measurement conditions of 25°C and 2 rpm. The lower limit of the above viscosity may be 20 Pa·s or 5 Pa·s. The upper limit of the above viscosity may be 75 Pa·s or 110 Pa·s. In the present disclosure, the viscosity of the composition is measured using an E-type viscometer. "rpm" is an abbreviation for "revolutions per minute."

[0094] In a preferred embodiment, the composition exhibits a viscosity within the range of 1 Pa·s to 60 Pa·s under measurement conditions of 25°C and 20 rpm. The lower limit of the viscosity may be 20 Pa·s or 5 Pa·s. The upper limit of the viscosity may be 30 Pa·s or 40 Pa·s.

[0095] In a preferred embodiment, the thixotropic index represented by the following formula is within a range of 0.5 to 7. The lower limit of the thixotropic index is preferably 0.6, more preferably 0.8, and even more preferably 1. The upper limit of the thixotropic index is preferably 4, more preferably 5, and even more preferably 6. Formula: Thixotropic index = ([viscosity of the composition obtained under the measurement conditions of 25°C and 2 rpm] ÷ [viscosity of the composition obtained under the measurement conditions of 25°C and 20 rpm]) × 100

[0096] (Method for producing composition) There is no limitation on the method for producing the composition as long as the target composition can be obtained. For example, the composition can be produced by mixing an epoxy resin, fumed silica, a curing accelerator, a thiol compound, and other components as needed.

[0097] (Purpose and Use of Composition) Examples of uses of the composition include casting agents, encapsulants, sealants, fiber-reinforced resins, coating agents, underfills, chip adhesives, electromagnetic wave shielding materials, coatings, and adhesives. In a preferred embodiment, the composition is used as an adhesive. The composition can be used, for example, as an adhesive for assembling electronic components. Examples of electronic components include camera modules, printed circuit boards, semiconductor devices, and integrated circuits. The electronic component can include a cured product of the composition. The composition can be injected between at least two electronic components, for example, between a semiconductor device and a substrate.

[0098] The composition can provide a cured product. For example, the composition can be cured by heat treatment. The heat treatment temperature is preferably in the range of 70°C to 150°C, more preferably 75°C to 120°C, and even more preferably 80°C to 100°C. The heat treatment time is preferably 1 minute to 60 minutes, more preferably 3 minutes to 45 minutes. Example

[0099] The present disclosure is described below based on examples. However, the present disclosure is not limited to the following examples. The following technical matters can be appropriately modified within the scope of the present disclosure.

[0100] <Manufacturing of Composition> A composition containing the components listed in Table 1 and Table 2 is manufactured according to the following steps. Epoxy resin and fumed silica are added to a dedicated container. Use a mixer (made by Nissin-based (Thinky) Co., Ltd., ARE-310) to thoroughly mix the epoxy resin and fumed silica at room temperature of 25°C and 2000 rpm for about 30 seconds to about 60 seconds, and then use a three-roll mill to knead them to obtain a dispersion. Add a latent curing accelerator to the dispersion. Use a mixer (made by Nissin-based Co., Ltd., ARE-310) to thoroughly mix the dispersion and the latent curing accelerator at room temperature of 25°C and 2000 rpm for about 30 seconds to about 60 seconds to obtain a masterbatch. Add a thiol compound to the masterbatch. Use a mixer (made by Nissin-based Co., Ltd., ARE-310) to mix the masterbatch and the thiol compound at room temperature of 25°C and 2000 rpm for about 20 seconds. The obtained mixture was degassed at 900 rpm for 2 minutes under vacuum using a stirring degasser (HM-200W, manufactured by Kyoritsu Seiki Co., Ltd.) to obtain a composition. For pressure control, the vacuum condition of the stirring degasser was set to "0".

[0101] The details of the materials of the composition are as follows. The names of the materials are represented by abbreviations of the compound names or product names. Unless otherwise specified, the viscosity is the viscosity at 25°C.

[0102] (Epoxy resin) "YL980": manufactured by Mitsubishi Chemical Corporation, bisphenol A epoxy resin, epoxy equivalent = 186 g / eq, viscosity = 13 Pa·s, molecular weight = 372 "YX7105": manufactured by Mitsubishi Chemical Corporation, flexible epoxy resin, epoxy equivalent = 489 g / eq, viscosity = 69 Pa·s, molecular weight = 978 "ZX-1059": Made by Nippon Steel Chemicals Co., Ltd., bisphenol A / bisphenol F epoxy resin, epoxy equivalent = 165 g / eq, viscosity = 2 Pa·s, molecular weight = 330 EXA-4850-150: manufactured by DIC Corporation, epoxy equivalent = 450 g / eq, viscosity = 15 Pa·s, molecular weight = 900

[0103] (Fumed Silica) RX300: Made by AEROSIL Co., Ltd., Japan. Fumed silica, surface modified with trimethylsilyl groups. Specific surface area = 180 m 2 / g~220m 2 / g, specific gravity = about 40g / L R976S: Made by AEROSIL Co., Ltd., Japan. Fumed silica, surface modified with dimethylsilyl groups. Specific surface area = 215 m 2 / g~265m2 / g, specific gravity = about 50g / L "R974": Made by AEROSIL Co., Ltd., Japan, fumed silica, surface modified with dimethylsilyl groups, specific surface area = 150 m 2 / g~190m 2 / g, specific gravity = about 50g / L RY300: Made by AEROSIL Co., Ltd., Japan. Fumed silica, surface treated with silicone oil. Specific surface area = 110 m 2 / g~140m 2 / g, specific gravity = about 50g / L RY200: Made by AEROSIL Co., Ltd., Japan. Fumed silica, surface treated with silicone oil. Specific surface area = 80 m 2 / g~120m 2 / g, specific gravity = about 50g / L R805: Made by AEROSIL Co., Ltd., Japan, fumed silica, surface modified with octylsilyl groups, specific surface area = 125 m 2 / g~175m 2 / g, specific gravity = 60g / L

[0104] (latent curing accelerator) "PN-23": Ajicure (registered trademark), manufactured by Ajinomoto Fine Technologies Co., Ltd., a solid-dispersion amine adduct-based latent curing accelerator "PN-40J": Ajicure (registered trademark), manufactured by Ajinomoto Fine Technologies Co., Ltd., a solid-dispersion amine adduct-based latent curing accelerator

[0105] (Thiol compound) "TMPIC": manufactured by Kawaguchi Chemical Industries, Ltd., tris(3-mercaptopropyl)isocyanurate, a trifunctional thiol having an isocyanuric acid skeleton, thiol equivalent = 117 g / eq, viscosity = 4.9 Pa·s, molecular weight = 351 "PE1": manufactured by RESONAC, pentaerythritol tetrakis(3-mercaptobutyrate), tetrafunctional secondary ester thiol, thiol equivalent = 136 g / eq, viscosity = 0.9 Pa·s, molecular weight = 544 "MR-123": manufactured by Daito Sangyo Co., Ltd., trifunctional non-ester thiol, thiol equivalent = 300 g / eq, viscosity = 14.2 Pa·s, molecular weight = 900 "PEPT" (Multhiol Y-3): manufactured by SC Organic Chemical Co., Ltd., a trifunctional thiol having a pentaerythritol skeleton, thiol equivalent = 124 g / eq, viscosity = 0.2 Pa·s, molecular weight = 372 “TMTP”: manufactured by Seishun Chemical Co., Ltd., trimethylolpropane tris(3-mercaptopropionate), trifunctional primary ester thiol, thiol equivalent = 140 g / eq, viscosity = 0.1 Pa·s, molecular weight = 420 "BD1": manufactured by RESONAC, 1,4-bis(3-mercaptobutyryloxy)butane, a difunctional secondary ester thiol, thiol equivalent = 147 g / eq, viscosity = 0.02 Pa·s, molecular weight = 147

[0106] The viscosity of each of the above thiol compounds was measured as follows: A rheometer (Thermo Fisher Scientific Inc., RheoStress 6000) was used as the viscosity measuring device. A cone-plate was used as the measuring fixture, and the shear rate was 400 s at 25°C. -1 The viscosity was measured using a 20 mm diameter cone and plate using C20 / 1-TiL. The distance between the cone tip and the plate was set to 0.052 mm, and a 0.04 mL sample was used.

[0107] <Determination of viscosity and thixotropic index> The temperature of the composition was maintained at 25°C, and the viscosity of the composition was measured using an E-type viscometer (RE-85U, manufactured by Toki Sangyo Co., Ltd.). The viscometer rotor was selected from the following three types based on the viscosity at 2 rpm. Specific measurement conditions are shown below. (1) Viscometer rotor: "1.34° × R24" (when the viscosity at 2 rpm is less than 20 Pa·s), "3° × R14" (when the viscosity at 2 rpm is 20 Pa·s or more and less than 50 Pa·s), or "3° × R9.7" (when the viscosity at 2 rpm is 50 Pa·s or more) (2) Speed: 2 rpm or 20 rpm (3) Measurement time: 2 minutes (4) Sample volume: 1.2 mL (1.34° × R24 rotor), 0.4 mL (3° × R14 rotor), or 0.22 mL (3° × R9.7 rotor)

[0108] Next, the thixotropic index was calculated according to the following formula. Formula: Thixotropic index = ([viscosity of the composition obtained under the measurement conditions of 25°C and 2 rpm] ÷ [viscosity of the composition obtained under the measurement conditions of 25°C and 20 rpm]) × 100

[0109] <Measurement of penetration width> The composition is filled into a dispenser syringe (Musashi Engineering, PSY-10E), then centrifugal degassing machine (Musashi Engineering, AWATRON3 AW-50-3) is used to carry out centrifugal degassing. Using an air distributor (Musashi Engineering, IMAGE MASTER 350PC Smart), the composition is applied on a copper substrate. Specifically, the composition is applied on a copper substrate so that the diameter of the composition on the substrate becomes about 500 μm. The surface roughness Ra of the copper substrate is 600 μm ± 50 μm. Then, using a thermal cycle oven (Yamataku Science (Yamato Scientific) company system, DF-610), the composition on the copper substrate is heated at 80 ° C for 30 minutes. Then, using a digital microscope (Keyence (Keyence) company system, VHX-7000) to observe the composition after heating, the maximum diameter of the composition after heating when measuring the top view and the maximum diameter of the infiltration material when looking down (the maximum diameter of the part where the component in the composition oozes out of the coating range of the composition). The width of each seepage material was calculated according to the following formula and the average value of 6 times was used for calculation: Formula: Width of seepage material = ([maximum diameter of seepage material] - [maximum diameter of the composition after heating]) ÷ 2

[0110] The width of the seepage material was evaluated according to the following criteria: A, B, and C were acceptable levels. A: less than 600μm B: 600 μm or more and less than 700 μm C: 700 μm or more and less than 800 μm D: 800μm or more

[0111] [Table 1]

[0112] [Table 2]

[0113] The compositions used in Examples 1-10 included fumed silica having at least one group selected from dimethylsilyl and trimethylsilyl groups, and a thiol compound exhibiting a viscosity of 0.2 Pa·s or greater at 25°C. As shown in Tables 1 and 2, Examples 1-10 achieved smaller bleed widths than Comparative Examples 1-8. In other words, Examples 1-10 suppressed bleed compared to Comparative Examples 1-8.

[0114] In Comparative Examples 1 and 2, which did not use a thiol compound exhibiting a viscosity of 0.2 Pa·s or greater at 25°C, the width of the bleed was large, and the occurrence of bleed could not be fully suppressed. In Comparative Examples 3 to 8, which did not use fumed silica having at least one group selected from a dimethylsilyl group and a trimethylsilyl group, the width of the bleed was large, and the occurrence of bleed could not be fully suppressed.

Claims

1. A composition, wherein Include: Epoxy resin, Fumed silica having at least one group selected from a dimethylsilyl group and a trimethylsilyl group, Curing accelerator, and A thiol compound having a viscosity of 0.2 Pa·s or more at 25°C.

2. The composition according to claim 1, wherein The viscosity of the thiol compound is within a range of 0.2 Pa·s to 15 Pa·s at 25°C.

3. The composition according to claim 1, wherein The content of the fumed silica is within a range of 0.1% by mass to 20% by mass based on the total mass of the composition.

4. The composition according to claim 1, wherein The content of the thiol compound is within a range of 1% by mass to 80% by mass based on the total mass of the composition.

5. The composition according to claim 1, wherein The thiol compound does not have a ring skeleton.

6. The composition according to claim 1, wherein The thiol compound has a ring skeleton.

7. The composition according to claim 1, wherein The thiol compound does not have an ester bond.

8. An adhesive, wherein: A composition comprising the composition according to any one of claims 1 to 7. 9 . A cured product, which is a cured product of the composition according to claim 1 .

10. An electronic component, wherein: The cured product according to claim 9 is included.

Citation Information

Cited By

  • High-performance yellowing-resistant TPU intermediate layer for laminated glass and preparation method thereof

    CN122080838A