Lubricant composition with wear resistance
By using a lubricant composition treated with modified sepiolite and silane coupling agent, the problems of poor stability and contamination of traditional lubricants in the metal wire drawing process are solved, achieving good dispersion and anti-wear properties of the lubricant, and reducing the cost and improve lubrication effect.
Patent Information
- Application Number
- CN202410639170.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-10-01
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricants, and in particular relates to a lubricant composition with anti-wear properties. Background Art
[0002] In the traditional metal cutting or wire drawing process, mineral oil, vegetable oil or cutting fluid is required as a lubricant for a large amount of flushing lubrication. The huge amount of usage not only wastes resources and causes huge pollution to the processing site and the environment, but also seriously affects the health of the operators.
[0003] Although there are many types of lubricants on the market, the lipid film formed by the lubricant on the surface of the workpiece is easily destroyed under normal working conditions, and deposits are easily formed during use, causing the friction pair to stick together and unable to work normally. In order to solve the above defects, many factories choose to add solid particles to the lubricant to increase the anti-wear performance of the lubricant, but adding too much solid particles will result in poor stability and serious deposition, and even aggravate the wear caused by friction during use.
[0004] CN201910587169.4 discloses a method for preparing a low-freezing point adipic acid ester diesel antiwear agent, wherein adipic acid, diol, triol and mixed fatty acid are put into a polyester reactor together, nitrogen is replaced and nitrogen is blasted to protect, so as to ensure that the reactor is always in a positive pressure state before vacuuming; the top temperature of the tower is controlled within 102°C, and the temperature is continuously raised to 230±2°C, and then kept warm for 3h; vacuuming is started, the vacuum degree is 0.02~0.04MPa, and the temperature is maintained at 230±2°C; when the acid value of the product drops to within 1.2mg KOH / g, the reaction is stopped, the temperature is lowered, the nitrogen blasting and the filter press are stopped. Compared with acid diesel antiwear agents, the product prepared by this patent using adipic acid as raw material can not only increase the wear resistance of diesel, but also conforms to the concept of environmental protection more and is non-corrosive to the engine and pipeline. This product has a good lubricating effect when applied to metal wire drawing, but the cost of using it alone is relatively high.
[0005] A large amount of waste liquid is generated during the metal drawing process, which usually contains a large amount of lubricating oil, metal debris and other impurities. If these waste liquids are not effectively treated, they will not only pollute the environment, but also waste resources. Summary of the invention
[0006] Purpose of the invention: In view of the problems that the additives in the current lubricants have poor stability and serious deposition during use, and the lipid film formed by the lubricant is easily destroyed, the present invention provides a lubricant composition with good dispersibility, good stability, low cost and anti-wear properties.
[0007] Specifically, the first aspect of the present disclosure is to provide a lubricant composition with anti-wear properties, which comprises the following raw materials in parts by weight: 80 to 90 parts of base oil, 7 to 11 parts of modified sepiolite, 3 to 8 parts of water, 2 to 5 parts of dispersant, and 1 to 3 parts of antioxidant.
[0008] In one embodiment, the base oil is obtained by treating wire drawing waste liquid.
[0009] In one embodiment, the method for treating the wire drawing waste liquid is to filter and decolorize the wire drawing waste liquid to remove impurities, and then add methanol to perform ester exchange to obtain base oil.
[0010] In one embodiment, the method for modifying sepiolite is to mix sepiolite and modifying liquid at a solid-liquid ratio of 3:7 to 10 g / mL, heat, spray dry, and ball-mill the dried particles and the synergist at a mass ratio of 9:1 to obtain modified sepiolite.
[0011] In one embodiment, the modified liquid is prepared by mixing a silane coupling agent and ethanol in a volume ratio of 3:8.
[0012] In one embodiment, the silane coupling agent is any one of vinyltrimethoxysilane, bis-[γ-(triethoxysilyl)propyl]tetrasulfide, and γ-aminopropyltriethoxysilane.
[0013] In one embodiment, the synergist is poly(p-hydroxybenzoic acid).
[0014] In one embodiment, the dispersant is any one of sodium polyacrylate and ammonium polyacrylate.
[0015] In one embodiment, the antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
[0016] The first aspect of the present disclosure provides application of the anti-wear lubricant composition in metal wire drawing.
[0017] Beneficial effects: The base oil of the present invention is obtained by treating wire drawing waste liquid. The wire drawing waste liquid is selected as the basic raw material. First, it can make full use of waste resources. Second, the cost is low. Third, the wire drawing waste liquid contains rich lipids and can have a good lubricating effect. The sepiolite modified by this method can make the sepiolite well dispersed in the lubricant, while ensuring stable performance, improving particle surface performance, preventing aggregation and precipitation, and increasing dispersibility and stability.
[0018] The above and other features, aspects and advantages of the present application will be more readily understood with reference to the following detailed description. DETAILED DESCRIPTION
[0019] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present disclosure belongs. In the event of a conflict, the definitions in this specification shall prevail.
[0020] Unless otherwise indicated, all percentages, parts, ratios, etc. are by weight.
[0021] As used herein, the terms "comprises," "comprising," "having," "having," "containing," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that includes a list of elements is not necessarily limited to those elements but may also include other elements not expressly listed or inherent to the composition, process, method, article, or apparatus.
[0022] When a quantity, weight portion or other numerical value or parameter is given as a range, a preferred range or a series of upper preferred values and lower preferred values, it should be understood that it specifically discloses all ranges formed by any pair of numerical values of any larger range limit or preferred value and any smaller range limit or preferred value, regardless of whether the range is disclosed separately. For example, when describing a range of "1 to 5", the described range should be understood to include a range of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. Unless otherwise stated, where a numerical range is described herein, the range is intended to include the range end value and all integers, fractions, decimals, etc. within the range.
[0023] In addition, the indefinite articles "a" and "an" before the elements or components of the present disclosure are intended to indicate that the number of occurrences (i.e., occurrences) of the elements or components is not limited. Therefore, "a" or "an" should be understood to include one or at least one, and unless it is clearly indicated that the number is singular, the elements or components in the singular form also include the plural case.
[0024] Unless specifically stated, the materials, methods, and examples described herein are illustrative only and not limiting. Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present disclosure, suitable methods and materials are still described herein.
[0025] The present disclosure is described in detail below.
[0026] A lubricant composition with anti-wear properties comprises the following raw materials in parts by weight: 80-90 parts of base oil, 7-11 parts of modified sepiolite, 3-8 parts of water, 2-5 parts of dispersant, and 1-3 parts of antioxidant.
[0027] The lubricant composition of the present invention has a good lubricating effect, and the modified sepiolite added therein has a good dispersing effect and good dispersibility, thereby increasing the wear resistance and enhancing the lubricity to a certain extent.
[0028] There is no particular limitation on the filler, which can be any of those conventionally used in the art. Advantageously, the base oil is obtained by treating wire drawing waste liquid. The wire drawing waste liquid is selected as the base raw material. First, waste resources can be fully utilized. Second, the cost is low. Third, the wire drawing waste liquid is rich in lipid substances, which can play a good lubricating effect.
[0029] There is no particular limitation on the treatment method of the wire drawing waste liquid, and it may be those conventionally used in the art. For example, the treatment method of the wire drawing waste liquid is to filter and decolorize the wire drawing waste liquid to remove impurities and odors to obtain pretreated oil, and then add methanol for ester exchange. During the ester exchange, a solid acid catalyst is added, wherein the amount of the solid acid catalyst added is 5-9% of the mass of methanol, and the solid acid catalyst is selected as silica-loaded ferric sulfate. The amount of methanol added is 13-16% of the volume of the pretreated oil to obtain a base oil.
[0030] For better effect, after removing impurities, the waste liquid is heated at 100-105°C for 30-40 minutes, and then the ester exchange is continued. The modified waste liquid obtained in this way has better lubrication effect.
[0031] Through high temperature treatment, a sterilization effect can be achieved, while some impurities can be removed, a certain proportion of moisture can be reduced, and the content of oil and fat can be increased.
[0032] For example, the filtration of wire drawing waste liquid can be carried out by using a screen or filtering equipment, and the filtration accuracy is: 1 micron. The filtration can be achieved through existing technology, and the main purpose is to remove impurities such as particles and floating objects.
[0033] For example, the decolorization of the wire drawing waste liquid can be achieved by combining activated carbon or kaolin with a flocculant, in order to further remove impurities such as pigments.
[0034] At the same time, the addition of solid acid in this process can play a catalytic role, allowing part of the grease to be pre-esterified in the wire drawing waste liquid, increasing the film-forming effect and then the lubrication effect, and it can also be recycled.
[0035] In the present invention, the method for modifying sepiolite is to mix sepiolite and a modifying liquid in a solid-liquid ratio of 3:7, heat at 60°C for 1 hour, spray dry, and ball-mill the dried particles and the synergist in a mass ratio of 9:1 to obtain the modified sepiolite. The sepiolite modified by the method can be well dispersed in the lubricant while ensuring stable performance.
[0036] The modified liquid used in the present invention is prepared by mixing a silane coupling agent and ethanol in a volume ratio of 3:8. The silane coupling agent is used to improve the surface properties of the particles, prevent aggregation and precipitation, and increase dispersibility and stability.
[0037] There is no particular limitation on the silane coupling agent, which may be any of those conventionally used in the art. Advantageously, the silane coupling agent is any one of vinyl trimethoxy silane, bis-[γ-(triethoxysilyl)propyl] tetrasulfide, and γ-aminopropyl triethoxy silane. The modification effect is better with these three. If further selection is made, vinyl trimethoxy silane is selected, which has the best effect.
[0038] As for the synergist, polyparahydroxybenzoic acid is selected in the present invention. The synergist can be used to enhance the dispersion effect of particles in one step, and enhance the lubricating effect and film-forming property of the lubricant.
[0039] There is no particular limitation on the dispersant, which may be any of those conventionally used in the art. Advantageously, the dispersant is any of sodium polyacrylate and ammonium polyacrylate.
[0040] There is no particular limitation on the antioxidant, which may be any of those conventionally used in the art. Advantageously, the antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol, which prevents the lubricant from oxidative deterioration during storage and enhances storage performance.
[0041] Example 1 Preparation of modified sepiolite 1
[0042] The silane coupling agent in the modified liquid is vinyl trimethoxy silane.
[0043] The method for modifying sepiolite is to mix sepiolite and modifying liquid at a solid-liquid ratio of 3:7 g / mL, heat to 60°C, and continue heating for 1 hour, spray dry, and ball mill the dried particles and the enhancer at a mass ratio of 9:1 to obtain modified sepiolite.
[0044] Example 2 Preparation of modified sepiolite 2
[0045] The silane coupling agent in the modified liquid is bis-[γ-(triethoxysilyl)propyl] tetrasulfide.
[0046] The method for modifying sepiolite is to mix sepiolite and modifying liquid at a solid-liquid ratio of 3:7 to 10 g / mL, heat to 60°C, and continue heating for 1 hour, spray dry, and ball mill the dried particles and the enhancer at a mass ratio of 9:1 to obtain modified sepiolite.
[0047] Example 3 Preparation of modified sepiolite 3
[0048] The silane coupling agent in the modified liquid is γ-aminopropyltriethoxysilane.
[0049] The method for modifying sepiolite is to mix sepiolite and modifying liquid evenly at a solid-liquid ratio of g / mL 3:7-10, heat to 60°C, and continue heating for 1 hour, spray dry, and ball-mill the dried particles and the enhancer at a mass ratio of 9:1 to obtain modified sepiolite.
[0050] Example 4 Preparation of a lubricant composition having anti-wear properties
[0051] The modified sepiolite 1 prepared in Example 1 was selected.
[0052] The dispersant is any one of sodium polyacrylate and ammonium polyacrylate.
[0053] The antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
[0054] A lubricant composition with anti-wear properties comprises the following raw materials in parts by weight: 80 parts of base oil, 7 parts of modified sepiolite 1, 3 parts of water, 2 parts of dispersant, and 1 part of antioxidant.
[0055] Example 5 Preparation of a lubricant composition having anti-wear properties
[0056] The modified sepiolite 2 prepared in Example 2 was selected.
[0057] The dispersant is any one of sodium polyacrylate and ammonium polyacrylate.
[0058] The antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
[0059] A lubricant composition with anti-wear properties comprises the following raw materials in parts by weight: 80 parts of base oil, 7 parts of modified sepiolite, 3 parts of water, 2 parts of dispersant and 1 part of antioxidant.
[0060] Example 6 Preparation of a lubricant composition having anti-wear properties
[0061] The modified sepiolite 3 prepared in Example 3 was selected.
[0062] The dispersant is any one of sodium polyacrylate and ammonium polyacrylate.
[0063] The antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
[0064] A lubricant composition with anti-wear properties comprises the following raw materials in parts by weight: 80 parts of base oil, 7 parts of modified sepiolite, 3 parts of water, 2 parts of dispersant and 1 part of antioxidant.
[0065] Example 7 Preparation of a lubricant composition having anti-wear properties
[0066] The modified sepiolite 1 prepared in Example 1 was selected.
[0067] The dispersant is any one of sodium polyacrylate and ammonium polyacrylate.
[0068] The antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
[0069] A lubricant composition with anti-wear properties comprises the following raw materials in parts by weight: 85 parts of base oil, 9 parts of modified sepiolite 1, 5 parts of water, 4 parts of dispersant, and 2 parts of antioxidant.
[0070] Example 8 Preparation of a lubricant composition having anti-wear properties
[0071] The modified sepiolite 1 prepared in Example 1 was selected.
[0072] The dispersant is any one of sodium polyacrylate and ammonium polyacrylate.
[0073] The antioxidant is any one of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
[0074] A lubricant composition with anti-wear properties comprises the following raw materials in parts by weight: 90 parts of base oil, 11 parts of modified sepiolite 1, 8 parts of water, 5 parts of dispersant, and 3 parts of antioxidant.
[0075] Comparative Example 1
[0076] It is basically the same as Example 4, except that the modified sepiolite is replaced by sepiolite.
[0077] Comparative Example 2
[0078] It is basically the same as Example 4, the only difference is that the modified sepiolite is replaced by the anti-wear agent prepared in Example 4 of CN201910587169.4 of the same mass.
[0079] Comparative Example 3
[0080] It is basically the same as Example 4, the only difference is that 1.5 parts of the anti-wear agent prepared in Example 4 of CN201910587169.4 are added.
[0081] The raw materials in Examples 4 to 8 and Comparative Examples 1 to 3 were mixed respectively and tested as follows:
[0082] According to the GB / T3142-2019 standard, a test steel ball with a diameter of 12.7 mm and a hardness of 65 was used. The test lasted for 1800 seconds under the conditions of a load of 500 N and a rotation speed of 1200 r / min. The friction coefficient and wear spot diameter were calculated. The results are as follows:
[0083]
[0084] Through the detection of the present invention, it can be obtained that the lubricant composition of the present invention has a good anti-wear effect.
[0085] The lubricant compositions prepared in Examples 4 to 8 and Comparative Examples 1 to 4 were subjected to stability tests. The stability test results at different temperatures and different storage times at room temperature are as follows:
[0086]
[0087] Note: √ represents maintaining the initial state, i.e. being stable; × represents becoming turbid or precipitating.
[0088] Through the detection of the present invention, it can be obtained that the lubricant composition of the present invention has good stability performance.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A lubricant composition having anti-wear properties, characterized in that: The composition comprises the following raw materials in parts by weight: 80-90 parts of base oil, 7-11 parts of modified sepiolite, 3-8 parts of water, 2-5 parts of dispersant and 1-3 parts of antioxidant.
2. The lubricant composition having anti-wear properties according to claim 1, characterized in that: The base oil is obtained by treating wire drawing waste liquid; the method for treating the wire drawing waste liquid comprises filtering and decolorizing the wire drawing waste liquid to remove impurities, and then adding methanol to perform ester exchange to obtain the base oil.
3. The lubricant composition having anti-wear properties according to claim 1, characterized in that: The preparation method of the modified sepiolite comprises the following steps: uniformly mixing sepiolite and a modifying liquid at a solid-liquid ratio of 3:7 to 10 g / mL, heating, spray drying, and ball milling the dried particles and a synergist at a mass ratio of 9:1 to obtain the modified sepiolite; the modifying liquid is prepared by mixing a silane coupling agent and ethanol at a volume ratio of 3:
8.
4. The lubricant composition having anti-wear properties according to claim 3, characterized in that: The silane coupling agent includes any one or more of vinyl trimethoxy silane, bis-[γ-(triethoxysilyl)propyl] tetrasulfide, and γ-aminopropyl triethoxy silane.
5. The lubricant composition having anti-wear properties according to claim 1, characterized in that: The synergist includes poly(p-hydroxybenzoic acid).
6. The lubricant composition having anti-wear properties according to claim 1, characterized in that: The dispersant is sodium polyacrylate and / or ammonium polyacrylate.
7. The lubricant composition having anti-wear properties according to claim 1, characterized in that: The antioxidant is any one or more of 2,6-di-tert-butyl-p-cresol and 2,4,6-tri-tert-butylphenol.
8. Use of the anti-wear lubricant composition according to any one of claims 1 to 7 in metal wire drawing.
Citation Information
Patent Citations
Method for preparing low freezing point adipate type diesel oil anti-wearing agent
CN110396444A