Method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing molten iron converter sticky slag phosphorus control technology
By adopting converter vanadium extraction, converter steelmaking and LF refining processes in vanadium-containing molten iron converter smelting, dynamically adjusting the vanadium extraction process and controlling oxygen lance parameters, the problems of excessive carbon oxidation and high-phosphorus weathering steel refining were solved, and high-phosphorus weathering steel was achieved. The low-cost smelting of weathering steel increases the added value of steel and resource utilization.
Patent Information
- Application Number
- CN202410746953.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
AI Technical Summary
During the converter smelting process of vanadium-containing molten iron, too rapid carbon oxidation leads to overoxidation, which affects the quality of steel. It is difficult to effectively refine high-phosphorus weathering steel with existing technology, and the refining efficiency of precious metals vanadium and titanium is low, resulting in a waste of resources.
Using converter extraction, converter steelmaking and LF refining processes, by dynamically adjusting the vanadium extraction process, controlling oxygen lance parameters, rationally adding dolomite and deoxidizer, increase the alkalinity in the ladle, reduce the amount of lime added, and use argon gas blowing and micro Positive pressure operation enables low-cost smelting of high-phosphorus weathering steel.
It has realized the low-cost smelting of high-phosphorus weathering steel, increased the added value of steel, saved mineral resources, reduced electricity consumption and smelting costs, and ensured the optimization of the chemical composition and structure of steel.
Smart Images

Figure BDA0004886717710000041 
Figure BDA0004886717710000051 
Figure BDA0004886717710000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for smelting high-phosphorus weathering steel at low cost by using a vanadium-containing molten iron converter slag sticking phosphorus control technology. Background Art
[0002] Weathering steel is a low-alloy steel with high corrosion resistance and toughness. It combines the properties of ordinary steel and stainless steel. By adding specific weather-resistant elements to its composition, this steel can form a dense oxide layer in the natural environment, which can effectively block the oxygen and moisture in the atmosphere from penetrating into the steel matrix, thereby slowing down the rust process and significantly improving the ability to resist atmospheric corrosion. It has a wide range of uses.
[0003] Chengde, as a vanadium-titanium resource base in my country, has rich vanadium-titanium resources. The ore contains vanadium with a grade of up to 0.3-0.7% and titanium with a grade of 5-6%. The grade of the selected vanadium-containing iron concentrate can reach 60-65%. There are many metals and minerals in the vanadium-titanium magnetite. Since the carbon content of vanadium-containing molten iron is lower than that of ordinary molten iron (carbon content of about 4.3%), the sulfur content is higher and the temperature is lower, the carbon content of vanadium-containing semi-steel is further reduced after vanadium extraction in the converter, and the heat-generating elements such as [Si] and [Mn] in the steel are oxidized into slag, and the heat-generating elements in the semi-steel are very low or even trace, which makes the semi-steel insufficient in heat, causing certain difficulties for converter smelting. Therefore, [C] begins to oxidize at the beginning of converter smelting, and the carbon oxidation reaches the maximum value within 3-5 minutes. The rapid increase in the carbon oxidation rate often causes overoxidation of molten steel and slag at the end of smelting. According to the above conditions, a method for controlling phosphorus in converter slag containing vanadium-containing molten iron to smelt high-phosphorus weathering steel at low cost is developed to solve the existing drawbacks and give full play to the advantages of molten iron smelting conditions of Chenggang to develop high-phosphorus weathering steel with a phosphorus content of 0.130-0.180%. The characteristic of weathering steel is that it needs to contain a certain amount of phosphorus in the steel, and can make full use of elements such as P, Cu, Ni, Cr in vanadium-containing molten iron. Phosphorus is a harmful element in ordinary steel grades. The necessary condition for dephosphorization is high alkalinity and large slag volume, which is conducive to phosphorus removal. Weathering steel requires a high phosphorus content. Since the dephosphorization task of steelmaking is reduced, the amount of lime added can be reduced, which can not only reduce costs but also increase the added value of steel. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for low-cost smelting of high-phosphorus weathering steel using vanadium-containing molten iron converter slag phosphorus control technology. The method includes converter vanadium extraction, converter steelmaking, and LF refining processes. While producing high-phosphorus weathering steel, the extraction of precious metals vanadium and titanium in vanadium-titanium molten iron is not affected, thereby saving mineral resources.
[0005] In order to solve the above technical problems, the technical scheme adopted by the present invention is as follows: a method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing molten iron converter slag sticking phosphorus control technology, the method comprising converter vanadium extraction, converter steelmaking, and LF refining processes; the converter vanadium extraction process: according to the carbon, temperature, silicon, titanium and vanadium elements of the molten iron, dynamic adjustment measures for vanadium extraction are formulated, and a target reverse blowing process is implemented to achieve dynamic adjustment of the vanadium extraction process, and crude oxygen is used for vanadium extraction, and a certain proportion of oxygen and nitrogen are mixed behind the oxygen lance cut-off valve to improve the stirring effect of the vanadium extraction molten pool; oxygen lance position control: the lance position is controlled at 1.25-1.50m, the nitrogen and oxygen pressure is controlled at 0.70-0.9Mpa, and the nitrogen flow rate is controlled at 10000-12000Nm 3 / h, oxygen flow rate 8000~11000Nm 3 / h, blowing time 4 to 8min, reaching semi-steel temperature 1345 to 1370℃, semi-steel carbon 3.2 to 3.4%, achieving the stability of semi-steel conditions.
[0006] The converter steelmaking process of the present invention comprises: adding copper plates and nickel plates into the furnace along with scrap steel and then adding them into molten iron for blowing; controlling the amount of dolomite added to be 10-20 kg / t steel; adding 2 / 3 of the total amount of dolomite in the early stage of blowing, and adding the rest in the later stage of blowing; controlling the bottom blowing argon flow rate to be 150-300 Nm 3 / h for blowing, controlling the oxygen pressure at 0.7~0.9Mpa, and the oxygen flow rate at 24000~36000Nm 3 / h; the oxygen lance slag gun position is controlled at 1.5-1.8 meters, the basic gun position is controlled at 1.4-1.6 meters, and the oxygen flow rate is 24000-26000Nm within 2 minutes before blowing 3 / h.
[0007] The converter steelmaking process of the present invention comprises the following steps: blowing for 11 to 15 minutes, the temperature of the molten steel being controlled at 1650 to 1670° C., after the blowing is completed, the steel grade requirements are met, steel tapping is organized, and the chemical composition melting range of the molten steel at the argon blowing station is: C: 0.05 to 0.07%, Si: 0.25 to 0.30%, Mn: 0.40 to 0.50%, P: 0.070 to 0.10%, S≤0.030%, Ni≤0.15%, Cu: 0.25 to 0.35%, Cr: 0.30 to 0.40%, ALs: 0.01 to 0.04%, [O]≤20ppm, and the remainder is Fe and unavoidable impurities.
[0008] The converter steelmaking process of the present invention comprises the following steps: the temperature of the first converter furnace at the end point is 1650-1670°C; the end point temperature of other furnaces is controlled at 1630-1650°C; after the ladle is seated, argon is blown from the bottom of the ladle to replace the gas in the ladle; 1.0-2.0 kg / t of deoxidizer Tai Aluminum is added during steel tapping; silicon-manganese alloy, ferrosilicon, low-carbon ferrochrome and ferrophosphorus are added when the steel tapping reaches 1 / 4-13; the steel tapping process requires that the steel be added evenly into the ladle; and the addition is completed when the steel tapping reaches 2 / 3-3 / 4 to avoid concentrated addition to impact the steel flow.
[0009] The converter steelmaking process of the present invention: the steel tapping time is controlled to be 4 to 8 minutes, the steel tapping process adopts an online argon blowing method, and after the steel tapping is completed, 0.85 to 1.71 kg / t of refined slag and 0.85 to 1.71 kg / t of small ash are added: the argon station blows argon for 2 to 3 minutes, and the argon flow rate is regulated to be 500 to 800 NL / min to fully stir and melt, control the FeO content in the ladle slag, and reduce the amount of oxygen transferred from the top slag to the molten steel during the lifting and casting process of the molten steel, thereby reducing the oxidation of the AL alloy element in the molten steel. After argon blowing, the temperature of the molten steel is ≥1600°C, and the argon station performs the ladle slag folding operation of the hot return slag in the continuous casting and the chemical composition requirements of the weathering steel grade are reused. The basicity of the slag in the ladle is increased to 3 to 4, the amount of refined lime added is reduced, and the cost is saved. The thickness of the slag layer is increased to ensure the arc buried effect of the electrode, improve the arc heat utilization rate, reduce the power consumption, save energy and reduce consumption, and increase the added value of product profits.
[0010] The LF refining process of the present invention comprises the following steps: the ladle is hoisted to the LF for smelting treatment, and after the ladle is seated, the argon gas is connected and adjusted to 500-1200NL / min for pre-purging argon, and a slightly positive pressure operation is adopted. The ladle is opened to the heating position, and the amount of deoxidizer aluminum powder added is adjusted according to the total aluminum and acid-soluble aluminum content of the chemical sample of the molten steel in the previous process, and 400-1000kg of slag lime and 200-300kg of aluminum ladle slag modifier are added. After the addition is completed, the argon gas is adjusted to increase the stirring power, improve the dynamic conditions, observe that the slag is completely melted, and adjust the argon gas to 150 ~300NL / min, select appropriate voltage power and 4 gears (short arc or long arc + foam slag) for heating operation. Appropriate slag thickness is conducive to arc burial, improves thermal efficiency, and reduces nitrogen absorption by molten steel. Stop heating after heating for 5-8 minutes, adjust the argon flow rate to improve the reaction ability of slag for deoxidation and desulfurization operations. During the process, dip the slag to observe the slag color, (alkalinity) state (black-yellow, green glass slag-white) and molten steel fluidity. Good fluidity is conducive to desulfurization reaction; timely adjust the amount of lime, fluorite, and aluminum powder added to adjust the slag until white slag is formed.
[0011] The LF refining process of the present invention comprises: controlling the acid-soluble aluminum in the molten steel according to the upper limit of the composition, adjusting the argon gas to 200-300NL / min and stirring for 2min to uniform the temperature and the composition; adjusting the argon gas to 30-80NL / min without exposing the liquid surface to perform calcium treatment and weakly blow argon for ≥10min to perform inclusion modification treatment and float the inclusions to the slag to purify the molten steel.
[0012] In the LF refining process of the present invention, the chemical composition and mass percentage of the molten steel at the refining endpoint are as follows: C: 0.07-0.10%, Si: 0.25-0.35%, Mn: 0.45-0.55%, P: 0.07-0.10%, S≤0.008%, Ni≤0.15%, Cu: 0.25-0.35%, Cr: 0.30-0.40%, Als: 0.01-0.04%, [N]≤40ppm, [O]≤30ppm, and other chemical residual elements are required to be: Nb+V+Ti≤0.22%, and the balance is Fe and unavoidable impurities.
[0013] In the converter steelmaking process of the present invention, the phosphorus content in the final molten steel is ≥50%. Phosphorus content = converter final phosphorus content / semi-steel initial phosphorus content*100%.
[0014] The beneficial effects of adopting the above technical scheme are as follows: the present invention studies the mechanism of dephosphorization and carries out slag sticking operation phosphorus control technology, so that the phosphorus content in the final molten steel of the converter reaches more than 50%; fully utilizes the advantages of elements such as P, Cu, Ni, Cr in the vanadium-containing molten iron to improve the product structure, saves the amount of cold material added during the converter smelting process, improves the basicity of the ladle slag, reduces the amount of refined lime added, and saves costs; increases the thickness of the slag layer, ensures the electrode buried arc effect, improves the arc heat utilization rate, reduces electricity consumption, saves energy, reduces consumption, and reduces smelting costs. DETAILED DESCRIPTION
[0015] The present invention is further described in detail below in conjunction with specific implementation modes.
[0016] Examples 1-8
[0017] A method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing hot metal converter slag phosphorus control technology, comprising converter vanadium extraction, converter steelmaking, and LF refining processes; each step is as follows:
[0018] 1) Converter vanadium extraction process: According to the carbon, temperature, silicon, titanium and vanadium elements in molten iron, formulate dynamic adjustment measures for vanadium extraction, implement the target reverse blowing process, realize dynamic adjustment of the vanadium extraction process, use crude oxygen to extract vanadium, and mix oxygen and nitrogen in a certain proportion behind the oxygen lance cut-off valve to improve the stirring effect of the vanadium extraction molten pool; oxygen lance position control: the lance position is controlled at 1.25-1.50m, the nitrogen and oxygen pressure is controlled at 0.70-0.9Mpa, and the nitrogen flow rate is controlled at 10000-12000Nm3 / h, oxygen flow rate 8000~11000Nm 3 / h, blowing time 4-8min, reaching semi-steel temperature 1345-1370°C, semi-steel carbon 3.2-3.4%, achieving stability of semi-steel conditions; the control parameters of the converter vanadium extraction process of Examples 1-8 are shown in Table 1.
[0019] Table 1 Control parameters of converter vanadium extraction process in Examples 1-8
[0020]
[0021] 2) Converter steelmaking process: copper plates and nickel plates are added into the furnace along with scrap steel and then added to molten iron for blowing. The amount of dolomite added is controlled at 10-20 kg / t steel. 2 / 3 of the total dolomite is added in the early stage of blowing, and the rest is added in the later stage of blowing. The bottom blowing argon flow rate is controlled at 150-300 Nm throughout the process. 3 / h for blowing, controlling the oxygen pressure at 0.7~0.9Mpa, and the oxygen flow rate at 24000~36000Nm 3 / h; the oxygen lance slag gun position is controlled at 1.5-1.8 meters, the basic gun position is controlled at 1.4-1.6 meters, and the oxygen flow rate is 24000-26000Nm within 2 minutes before blowing 3 / h;
[0022] Blowing for 11 to 15 minutes, the temperature of the molten steel is controlled at 1650 to 1670°C. After blowing, the steel grade requirements are met and steel tapping is organized. The chemical composition melting range of the molten steel at the argon blowing station is controlled as follows: C: 0.05 to 0.07%, Si: 0.25 to 0.30%, Mn: 0.40 to 0.50%, P: 0.070 to 0.10%, S≤0.030%, Ni≤0.15%, Cu: 0.25 to 0.35%, Cr: 0.30 to 0.40%, ALs: 0.01 to 0.04%, [O]≤20ppm, the remainder is Fe and unavoidable impurities;
[0023] The temperature of the first furnace at the end of the converter is 1650-1670℃; the end temperature of other furnaces is controlled at 1630-1650℃. After the ladle is seated, argon is blown from the bottom of the ladle to replace the gas in the ladle. The deoxidizer Tai Aluminum 1.0-2.0 kg / t steel is added during the tapping. When the tapping reaches 1 / 4-13, silicon-manganese alloy, ferrosilicon and low-carbon ferrochrome are added. It is required that the steel is added evenly into the ladle during the tapping process and the addition is completed when the tapping reaches 2 / 3-3 / 4 to avoid concentrated addition to impact the steel flow.
[0024] The steel-tapping time is controlled to be 4 to 8 minutes, and the steel-tapping process adopts the online argon blowing method. After the steel-tapping is completed, 0.85 to 1.71 kg / t of refined slag and 0.85 to 1.71 kg / t of small ash are added: the argon station blows argon for 2 to 3 minutes, and the argon flow rate is adjusted to 500 to 800 NL / min to fully stir and melt, control the FeO content in the ladle slag, and reduce the amount of oxygen transferred from the top slag to the molten steel during the lifting and casting process of the molten steel, thereby reducing the oxidation of the AL alloy elements in the molten steel. After argon blowing, the temperature of the molten steel is ≥1600°C, and the argon station performs the ladle slag folding operation of the hot return slag of continuous casting and the chemical composition requirements of the weathering steel grade are met. Increase the basicity of the ladle slag to 3 to 4, reduce the amount of refined lime added, and save costs. Increase the thickness of the slag layer, ensure the arc buried effect of the electrode, improve the arc heat utilization rate, reduce the power consumption, save energy and reduce consumption, and increase the product profit added value; the control parameters of the converter steelmaking process of Examples 1-8 are shown in Table 2.
[0025] Table 2 Control parameters of converter steelmaking process in Example 1-8
[0026]
[0027] In Table 2, Examples 1-5 are the first heat of the converter, and Examples 6-8 are the other heats of the converter.
[0028] Table 2 Control parameters of converter steelmaking process in Example 1-8
[0029]
[0030] 3) LF refining process: The ladle is hoisted to LF for smelting treatment. After the ladle is seated, the argon gas is connected and adjusted to 500-1200NL / min for pre-purging of argon. The ladle is operated with a slight positive pressure. The ladle is opened to the heating position. According to the total aluminum and acid-soluble aluminum content of the chemical sample of the molten steel in the previous process, the amount of deoxidizer aluminum powder added is adjusted. 400-1000kg of slag lime and 200-300kg of aluminum ladle slag modifier are added. After the addition is completed, the argon gas is adjusted to increase the stirring power and improve the dynamic conditions. Observe that the slag is completely melted, and adjust the argon gas to 150-2000Nl / min. 300NL / min, select appropriate voltage power and 4 gears (short arc or long arc + foam slag) for heating operation. Appropriate slag thickness is conducive to arc burial, improves thermal efficiency, and reduces nitrogen absorption by molten steel. Stop heating after heating for 5 to 8 minutes, adjust the argon flow rate to improve the reaction ability of slag for deoxidation and desulfurization operations. During the process, dip the slag to observe the slag color, (alkalinity) state (black-yellow, green glass slag-white) and molten steel fluidity. Good fluidity is conducive to desulfurization reaction; timely adjust the amount of lime, fluorite, and aluminum powder added to adjust the slag until white slag is formed.
[0031] The acid-soluble aluminum in the molten steel is controlled according to the upper limit of the composition, and the argon gas is adjusted to 200-300NL / min and stirred for 2min to make the temperature and composition uniform; the argon gas is adjusted to 30-80NL / min without exposing the liquid surface for calcium treatment and weak argon blowing for ≥10min, and the inclusions are denatured and floated to the slag to purify the molten steel; the control parameters of the LF furnace refining step of Example 1-8 are shown in Table 3, and the chemical composition of the molten steel is shown in Table 4.
[0032] Table 3 LF refining process control parameters in Examples 1-8
[0033]
[0034]
[0035] In Table 3, the argon flow rate corresponds to the argon flow rate control of the above-mentioned LF furnace refining step in chronological order.
[0036] Table 4 Chemical composition and mass percentage of molten steel at the end point of LF refining in Example 1-8
[0037]
[0038] 4) Continuous casting process: The molten steel refined in the LF furnace is continuously cast, and the remaining slag in the continuous casting ladle is folded into a ladle and poured into the argon station ladle.
[0039] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology, characterized in that: The method comprises converter vanadium extraction, converter steelmaking and LF refining process; the converter vanadium extraction process: oxygen lance position control: the lance position is controlled at 1.25-1.50m, the nitrogen and oxygen pressure is controlled at 0.70-0.9Mpa, and the nitrogen flow rate is controlled at 10000-12000Nm 3 / h, oxygen flow rate 8000~11000Nm 3 / h, blowing time 4 to 8min, reaching semi-steel temperature 1345 to 1370℃, semi-steel carbon 3.2 to 3.4%.
2. The method for smelting high-phosphorus weathering steel with low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology according to claim 1, characterized in that: The converter steelmaking process: copper plates and nickel plates are added into the furnace along with scrap steel and then added into molten iron for blowing; the dolomite addition amount is controlled to be 10-20 kg / t steel; 2 / 3 of the total dolomite is added in the early stage of blowing, and the rest is added in the later stage of blowing; the bottom blowing argon flow rate is controlled to be 150-300 Nm 3 / h for blowing, controlling the oxygen pressure at 0.7~0.9Mpa, and the oxygen flow rate at 24000~36000Nm 3 / h; the oxygen lance slag gun position is controlled at 1.5-1.8 meters, the basic gun position is controlled at 1.4-1.6 meters, and the oxygen flow rate is 24000-26000Nm within 2 minutes before blowing 3 / h.
3. The method for smelting high-phosphorus weathering steel with low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology according to claim 1, characterized in that: The converter steelmaking process comprises: blowing for 11 to 15 minutes, the temperature of the molten steel is controlled at 1650 to 1670° C. After the blowing is completed, the steel grade requirements are met and steel tapping is organized. The chemical composition melting range of the molten steel at the argon blowing station is: C: 0.05 to 0.07%, Si: 0.25 to 0.30%, Mn: 0.40 to 0.50%, P: 0.070 to 0.10%, S≤0.030%, Ni≤0.15%, Cu: 0.25 to 0.35%, Cr: 0.30 to 0.40%, ALs: 0.01 to 0.04%, [O]≤20ppm, and the remainder is Fe and unavoidable impurities.
4. The method for smelting high-phosphorus weathering steel at low cost by using a vanadium-containing hot metal converter slag sticking phosphorus control technology according to any one of claims 1 to 3, characterized in that: The converter steelmaking process comprises the following steps: the temperature of the first converter furnace at the end point is 1650-1670°C; the end point temperature of other furnaces is controlled at 1630-1650°C; after the ladle is seated, argon is blown from the bottom of the ladle to replace the gas in the ladle; 1.0-2.0 kg / t of deoxidizer Tai Aluminum is added during steel tapping; silicon-manganese alloy, ferrosilicon and low-carbon ferrochrome are added when the steel tapping reaches 1 / 4-13; and the addition is completed when the steel tapping reaches 2 / 3-3 / 4.
5. The method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology according to any one of claims 1 to 3, characterized in that: The converter steelmaking process: the steel tapping time is controlled at 4 to 8 minutes, the steel tapping process adopts an online argon blowing method, and after the steel tapping is completed, 0.85 to 1.71 kg / t of refined slag and 0.85 to 1.71 kg / t of small-grained lime are added: the argon station blows argon for 2 to 3 minutes, and the argon flow rate is regulated at 500 to 800 NL / min for sufficient stirring and melting. After the argon blowing, the temperature of the molten steel is ≥1600°C, and the basicity of the slag in the ladle is increased to 3 to 4.
6. The method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology according to any one of claims 1 to 3, characterized in that: The LF refining process includes: the ladle is hoisted to the LF for smelting treatment, and after the ladle is seated, the argon is connected and adjusted to 500-1200NL / min for pre-purging argon, and a slightly positive pressure operation is adopted. The ladle is opened to the heating position, and the amount of deoxidizer aluminum powder added is adjusted according to the total aluminum and acid-soluble aluminum content of the molten steel chemical sample in the previous process, and 400-1000kg of slag lime and 200-300kg of aluminum ladle slag modifier are added. After the addition is completed, the argon is adjusted to increase the stirring power, and the argon is adjusted to 150-300NL / min to observe that the slag is completely melted.
7. A method for smelting high-phosphorus weathering steel at low cost by using a vanadium-containing hot metal converter slag sticking phosphorus control technology according to any one of claims 1 to 3, characterized in that: The LF refining process comprises: controlling the acid-soluble aluminum in the molten steel according to the upper limit of the composition, adjusting the argon gas to 200-300NL / min and stirring for 2 minutes to uniform the temperature and composition; adjusting the argon gas to 30-80NL / min and weakly blowing argon for ≥10 minutes without exposing the liquid surface for calcium treatment.
8. The method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology according to any one of claims 1 to 3, characterized in that: In the LF refining process, the chemical composition and mass percentage of the molten steel at the refining endpoint are as follows: C: 0.07-0.10%, Si: 0.25-0.35%, Mn: 0.45-0.55%, P: 0.07-0.10%, S≤0.008%, Ni≤0.15%, Cu: 0.25-0.35%, Cr: 0.30-0.40%, Als: 0.01-0.04%, [N]≤40ppm, [O]≤30ppm, and other chemical residual elements are required to be: Nb+V+Ti≤0.22%, and the balance is Fe and unavoidable impurities.
9. The method for smelting high-phosphorus weathering steel at low cost by using vanadium-containing hot metal converter slag sticking phosphorus control technology according to any one of claims 1 to 3, characterized in that: In the converter steelmaking process, the phosphorus content in the final molten steel is ≥50%.