Gradient extraction method for metal in arsenic-containing material
Through gradient leaching method and Fe3+ ion regulation, the problem of difficult control of As leaching behavior in hydrometallurgy is solved, efficient recovery of valuable metals is achieved, As removal burden and process cost are reduced, and it is suitable for the treatment of refractory minerals.
Patent Information
- Application Number
- CN202410860566.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
In the hydrometallurgical process, it is difficult to effectively control the leaching behavior of arsenic elements in arsenic-containing materials, resulting in excessive As content in the system, which increases the burden of arsenic removal and equipment maintenance costs. The existing As removal methods are not suitable for high As concentration solutions. It is applicable, and the treatment process has safety hazards and high energy consumption issues.
Gradient leaching method is adopted, through low-acid and high-acid leaching treatment steps, combined with Fe3+ ions and pH adjustment, to control the precipitation of As and the extraction of valuable metals, reduce the entry of As into the solution system, reduce the burden of As removal, and improve the metal recovery rate .
It achieves leaching out as much valuable metal as possible under low As leaching conditions, reducing the entry of As into the solution system, reducing the burden of As removal, improving the metal recovery rate and the economy and operating efficiency of the process, and is suitable for the treatment of refractory minerals .
Smart Images

Figure CN118726749A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for gradient extraction of metals from arsenic-containing materials. Background Art
[0002] Arsenic is widely present in nonferrous metal and precious metal minerals in the form of arsenopyrite (FeAsS), copper arsenic sulfide (Cu3AsS4), arsenic iron (FeAs), realgar (As2S2) and orpiment (As2S3) in nature. Against the backdrop of resource shortages, the development of refractory resources has become an increasingly popular trend, with copper, zinc and lead mineral resources containing As being the most typical. Taking the smelting process of zinc ore containing As as an example, a large amount of zinc oxide dust containing As will be produced after pyrometallurgical smelting. During this process, As is enriched. The As in this part of the dust is even several times higher than the As content in the ore. In the subsequent wet leaching process, this part of As tends to be leached together with zinc, causing the As content in the system to exceed the standard (up to ~20 g / L). This problem also exists in the smelting of other valuable metals (including tin, lead, copper, etc.). A large amount of As enters the solution system, which will have a severe impact on the energy consumption of the process, equipment maintenance, and product quality. How to control the leaching behavior of As in the hydrometallurgical process, reduce the burden of subsequent arsenic removal, and reduce the amount of arsenic removal slag are issues that need to be addressed urgently.
[0003] At present, the main methods for removing arsenic from solutions include physical As removal methods such as membrane separation and adsorption, and chemical As removal methods such as sulfidation, oxidation, and reduction. Among them, physical As removal methods are mainly aimed at deep As removal where the As concentration is less than 1g / L, and are not applicable to the As removal requirements of hydrometallurgy that are often more than 10g / L. In the field of hydrometallurgy, chemical As removal methods are mainly used to treat solutions. The sulfidation method mainly adds sodium sulfide or hydrogen sulfide to the solution to combine with As to form arsenic sulfide to achieve the purpose of arsenic removal. The reduction method is common in copper smelting arsenic removal, mainly in the form of Cu3As precipitation to achieve the purpose of arsenic removal. The sulfidation method requires the use of sulfides, which are highly toxic and have a harsh operating environment, which limits its application. The reduction method has higher requirements on the composition of the solution, requiring the solution to be Cu3As. 2+ and As 2+ The molar ratio of As to Fe is not less than 3, so its application is limited. The oxidation method generally uses an oxidant to oxidize As in the solution into pentavalent As, and then introduces Fe 3+ or Ca 2+ The metal cations such as arsenate are precipitated to achieve the purpose of arsenic removal. The oxidation method is the most applicable and effective method in hydrometallurgy among the many arsenic removal methods currently available.
[0004] As an extremely important source of difficult-to-treat minerals, the development of As-containing mineral processing technology will become an unavoidable issue in the context of the gradual shift of resource development to difficult-to-treat minerals. How to economically and effectively recover valuable metals from these minerals has very important economic value and social significance for energy conservation and consumption reduction in the non-ferrous metal industry and solving the three waste problems. Summary of the invention
[0005] The object of the present invention is to provide a method for gradient extraction of metals from arsenic-containing materials, so as to efficiently recover the metals from the arsenic-containing materials.
[0006] The above purpose can be achieved by implementing the following technical solutions:
[0007] A method for gradient extraction of metals from arsenic-containing materials comprises the following steps:
[0008] Step 1) low-acid leaching: adding sulfuric acid to the arsenic-containing metallurgical material for leaching treatment, with an acid-ore ratio of 500-550 kg / t and a liquid-solid ratio of 4:1-6:1 to obtain a low-acid leaching solution and a low-acid leaching slag;
[0009] Step 2) high acid leaching: adding sulfuric acid to the low acid leaching residue for leaching treatment, with an acid-ore ratio of 200-300 kg / t and a liquid-solid ratio of 2:1-4:1 to obtain a high acid leaching solution and high acid leaching residue;
[0010] Step 3) Add Fe to the high acid leaching solution 3+ , controlling the Fe / As ratio to 0.1-1 and adjusting the pH of the high-acid leaching solution to 1.5-5.0 to react and precipitate arsenic to obtain arsenic removal slag and arsenic removal liquid; extracting metal ions from the arsenic removal liquid and the low-acid leaching solution.
[0011] Optionally, in step 3), the pH of the high-acid leaching solution is adjusted using hydroxide of the extracted metal ions.
[0012] Optionally, in the step 1), the low acid leaching reaction time is 1 to 6 hours and the reaction temperature is 70-90° C.;
[0013] The high acid leaching reaction time in the step 2) is 1 to 6 hours and the reaction temperature is 70-90°C.
[0014] Optionally, the arsenic-removed slag is returned to the low-acid leaching slag in step 2) for leaching treatment again.
[0015] Optionally, in step 3, Fe 3+ At least one of Fe2(SO4)3, FeCl3 or Fe(NO3)3 is used.
[0016] Optionally, in step 3), the reaction time is 1 to 4 hours and the reaction temperature is 70-90°C.
[0017] Optionally, the arsenic-containing metallurgical material is arsenic-containing smoke.
[0018] Optionally, in the step 3), zinc ions and / or copper ions in the arsenic-removed liquid and the low-acid leaching liquid are extracted.
[0019] Optionally, the leaching end point H of the low-acid leaching solution in step 1) is + Concentration: 0.01-0.05mol / L.
[0020] Optionally, the leaching end point H of the high acid leaching solution in step 2) is + Concentration: 0.45-0.75mol / L.
[0021] The technical solution of the invention has the following advantages:
[0022] The method of the present invention treats arsenic-containing materials through a gradient leaching method of low-acid leaching and high-acid leaching. Under the condition of first leaching less As or even no leaching, the valuable metals are leached as much as possible, and then under the condition of controlling the leaching of all valuable metals, the segmented leaching method of As leaching is minimized to reduce the entry of As into the solution system and reduce the burden of As removal. The method of the present invention comprehensively considers the destination of As and valuable metals in the entire leaching system, the feasibility of As removal, the selection of neutralizers, etc. The optimized parameters can guide actual production, and the metal recovery rate is high, the compatibility with materials is good, and it is easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 It is the process flow chart of Example 1;
[0025] Figure 2 This is the element weight flow chart of Example 1. DETAILED DESCRIPTION
[0026] Now, various exemplary embodiments of the present invention are described in detail, which should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0027] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0028] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0029] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0030] The present invention proposes a gradient treatment method for As-containing materials. The As-containing smoke dust is used as a raw material, and a low-As leaching solution and a low-acid leaching slag are prepared by a low-acid leaching reaction. The low-As leaching solution directly enters a clean liquid system without the need for As removal. The low-acid leaching slag is further subjected to high-acid leaching to leach all the valuable metals in the slag, thereby obtaining a high-acid leaching solution and a high-acid leaching slag. The high-acid leaching slag is stored because the valuable metal content is extremely low and As also mainly exists in a difficult-to-leach form. The high-acid leaching solution contains a certain amount of As in addition to the valuable metals, so As needs to be removed. An alkaline solution consistent with the main valuable metals in the high-acid leaching solution is used to remove the As. 3+ The solution is added to remove As, and As-removed slag and As-removed liquid are obtained. Depending on the valuable metal content in the As-removed slag, it is decided whether to further return the As-removed slag for high-acid leaching to recover the valuable metals. This process can recover the valuable metals in the As-containing materials to the greatest extent, while effectively reducing the burden of As removal, and effectively improving the economy and operating efficiency of the As-containing material treatment process.
[0031] Example 1
[0032] like Figure 1 As shown in the figure, the As-containing zinc oxide dust was subjected to low-acid leaching under the conditions of acid-ore ratio of 530 kg / t, liquid-solid ratio of 5:1, reaction time of 2 h, and reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain low-As leaching solution (As concentration was less than 0.005 g / L) and low-acid leaching residue. The leaching rates of As and Zn were 0.03% and 82.87%, respectively. + The concentration is 0.04mol / L.
[0033] The low-acid leaching residue was subjected to high-acid leaching under the conditions of acid-ore ratio of 225 kg / t, liquid-solid ratio of 3:1, reaction time of 1 h, and reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain high-acid leaching solution and high-acid leaching residue. The leaching rates of As and Zn were ~74.77% and ~100.64%, respectively. The high-acid leaching solution contained a certain amount of As, and the filtrate concentration was ~27.5 g / L, so As removal was required. The high-acid leaching residue contained almost no Zn, and As also existed mainly in a difficult-to-leach form. Considering storage or extraction of other valuable metals (such as Pb). + The concentration is 0.50mol / L.
[0034] Fe 3+ The salt saturated solution and the high-acid leaching solution are added to the main metal hydroxides in the flue dust to control the solution pH, and As is removed under the conditions of pH 2.0, Fe / As ratio 0.3641, reaction time 4h, and reaction temperature 90°C. Further liquid-solid separation is performed to obtain As-removed slag and As-removed liquid. The concentration of the filtrate after As removal is 0.3g / L, the As liquid removal rate is ~92.93%, and the Zn liquid loss rate is ~6.39%. The As content in the As-removed liquid is low, and it can directly enter the clean liquid process for subsequent extraction of valuable metals. The As-removed slag contains a certain amount of Zn and can be returned to the high-acid leaching process for further extraction of Zn.
[0035] The slag after As removal is subjected to high-acid leaching at an acid-ore ratio of 225 kg / t, a liquid-solid ratio of 3:1, a reaction time of 1 h, and a reaction temperature of 90°C. Further liquid-solid separation is performed to obtain high-acid leaching liquid and high-acid leaching slag. The As and Zn liquid-based leaching rates are 21.00% and 74.60%, respectively.
[0036] Figure 2 As and Zn element trend diagram. Assuming that the smoke contains 10g As and 100g Zn, it is roughly estimated that the amount of Zn metal entering the slag in the process does not exceed 1g, accounting for less than 1% of the total Zn metal amount in the system, that is, the total recovery rate of Zn in this process is above 99%.
[0037] Example 2
[0038] The zinc oxide dust containing As was subjected to low-acid leaching under the conditions of acid-ore ratio of 500 kg / t, liquid-solid ratio of 6:1, reaction time of 1 h, and reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain low-As leaching solution (As concentration of 0.001 g / L) and low-acid leaching residue. The leaching rates of As and Zn were 0.01% and 80.00%, respectively. + The concentration is 0.02mol / L.
[0039] The low-acid leaching residue was subjected to high-acid leaching at an acid-ore ratio of 300 kg / t, a liquid-solid ratio of 4:1, a reaction time of 1 h, and a reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain high-acid leaching solution and high-acid leaching residue. The leaching rates of As and Zn were 71.13% and 94.13%, respectively. + The concentration is 0.69mol / L.
[0040] Fe 3+ The salt saturated solution and the high-acid leaching solution are added to the main metal hydroxides in the flue dust to control the solution pH, and As is removed under the conditions of pH 2.0, Fe / As ratio 0.1, reaction time 4h, and reaction temperature 90°C. Further liquid-solid separation is performed to obtain As-removed slag and As-removed liquid. The As content in the As-removed liquid is low, and it can directly enter the clean liquid process for subsequent extraction of valuable metals. The As-removed slag contains a certain amount of Zn and can be returned to the high-acid leaching process for further extraction of Zn.
[0041] Example 3
[0042] The zinc oxide dust containing As was subjected to low-acid leaching at an acid-ore ratio of 530 kg / t, a liquid-solid ratio of 6:1, a reaction time of 1 h, and a reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain a low-As leaching solution (As concentration 0.0139 g / L) and low-acid leaching residue. The leaching rates of As and Zn were 0.11% and 78.34%, respectively. + The concentration is 0.01mol / L.
[0043] The low-acid leaching residue was subjected to high-acid leaching at an acid-ore ratio of 200 kg / t, a liquid-solid ratio of 4:1, a reaction time of 1 h, and a reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain high-acid leaching solution and high-acid leaching residue. The leaching rates of As and Zn were 64.87% and 87.34%, respectively. The high-acid leaching solution had a filtrate concentration of 13.82 g / L due to the presence of a certain amount of As. + The concentration is 0.34mol / L.
[0044] Fe 3+ The salt saturated solution and the high-acid leaching solution are added to the main metal hydroxides in the flue dust to control the solution pH, and As is removed under the conditions of pH 2.0, Fe / As ratio 1, reaction time 1h, and reaction temperature 70°C. Further liquid-solid separation is performed to obtain As-removed slag and As-removed liquid. The As content in the As-removed liquid is low, and it can directly enter the clean liquid process for subsequent extraction of valuable metals. The As-removed slag contains a certain amount of Zn and can be returned to the high-acid leaching process for further extraction of Zn.
[0045] Comparative Example 1
[0046] The zinc oxide dust containing As is directly subjected to high acid leaching under the conditions of acid-ore ratio of 1488 kg / t, liquid-solid ratio of 2:1, reaction time of 1 h, and reaction temperature of 90°C. After liquid-solid separation, a leachate with an As concentration of up to 39.93 g / L and a leaching residue with a Zn content of 23.59% can be obtained. The leaching rates of As and Zn are 82.70% and 83.65%, respectively. Even if the optimized As removal conditions are used for As removal, the total Zn recovery rate of the process is less than 82%.
[0047] Comparative Example 2
[0048] The As-containing zinc oxide dust was subjected to low-acid leaching under the conditions of acid-ore ratio of 530 kg / t, liquid-solid ratio of 3:1, reaction time of 1 h, and reaction temperature of 90 °C. Further liquid-solid separation was performed to obtain As-containing leaching solution (As concentration of 0.1598 g / L) and low-acid leaching residue. + The concentration is 0.02mol / L. The leaching rates of As and Zn are 0.46% and 76.46%, respectively. It can be seen that the concentration of As is 50 times that of the low-acid leaching solution in Example 1, and the As leaching solution is 15 times that of Example 1. If this part of the solution is directly entered into the purification process without treatment, it is inevitable that the arsenic in the system will accumulate rapidly, affecting the smooth process. If it is treated, the arsenic removal load of the system will be increased, making the process economy worse.
[0049] Comparative Example 3
[0050] The As-containing zinc oxide dust was subjected to low-acid leaching under the conditions of acid-ore ratio of 100 kg / t, liquid-solid ratio of 5:1, reaction time of 1 h, and reaction temperature of 90 °C. + The concentration is very low (pH 5.95), As is not leached and the leaching rate of Zn is only 13.70%.
[0051] Comparative Example 4
[0052] The As-containing zinc oxide dust was subjected to low-acid leaching at an acid-ore ratio of 200 kg / t, a liquid-solid ratio of 5:1, a reaction time of 1 h, and a reaction temperature of 90 °C. + The concentration of As was very low (pH 5.88). As was not leached and the leaching rate of Zn was only 25.50%.
[0053] Comparative Example 5
[0054] The As-containing zinc oxide dust was subjected to low-acid leaching under the conditions of acid-ore ratio of 800 kg / t, liquid-solid ratio of 6:1, reaction time of 1 h, and reaction temperature of 90 °C. + The concentration is 0.38 mol / L. The As leaching rate is as high as 89.48%, and Zn is almost completely leached.
[0055] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A gradient extraction method for metals in arsenic-containing materials, characterized in that: The steps include: Step 1) low-acid leaching: adding sulfuric acid to the arsenic-containing metallurgical material for leaching treatment, with an acid-ore ratio of 500-550 kg / t and a liquid-solid ratio of 4:1-6:1 to obtain a low-acid leaching solution and a low-acid leaching slag; Step 2) high acid leaching: adding sulfuric acid to the low acid leaching residue for leaching treatment, with an acid-ore ratio of 200-300 kg / t and a liquid-solid ratio of 2:1-4:1 to obtain a high acid leaching solution and high acid leaching residue; Step 3) Add Fe to the high acid leaching solution 3+ , controlling the Fe / As ratio to 0.1-1 and adjusting the pH of the high-acid leaching solution to 1.5-5.0 to react and precipitate arsenic to obtain arsenic removal slag and arsenic removal liquid; extracting metal ions from the arsenic removal liquid and the low-acid leaching solution.
2. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: In the step 3), the pH of the high-acid leaching solution is adjusted using the hydroxide of the extracted metal ions.
3. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: In the step 1), the low-acid leaching reaction time is 1 to 6 hours and the reaction temperature is 70-90° C.; The high acid leaching reaction time in the step 2) is 1 to 6 hours and the reaction temperature is 70-90°C.
4. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: The arsenic-removed slag is returned to the low-acid leaching slag in step 2) for further leaching treatment.
5. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: In the step 3, Fe 3+ At least one of Fe2(SO4)3, FeCl3 or Fe(NO3)3 is used.
6. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: In the step 3), the reaction time is 1 to 4 hours and the reaction temperature is 70-90°C.
7. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: The arsenic-containing metallurgical material is arsenic-containing smoke.
8. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: In the step 3), the zinc ions and / or copper ions in the arsenic-removed solution and the low-acid leaching solution are extracted.
9. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: The leaching end point H of the low-acid leaching solution in step 1) + Concentration: 0.01-0.05mol / L.
10. The method for gradient extraction of metals from arsenic-containing materials according to claim 1, characterized in that: The leaching end point H of the high acid leaching solution in step 2) + Concentration: 0.45-0.75mol / L.